CN1079769A - 建筑隔热防水粉 - Google Patents

建筑隔热防水粉 Download PDF

Info

Publication number
CN1079769A
CN1079769A CN 92108160 CN92108160A CN1079769A CN 1079769 A CN1079769 A CN 1079769A CN 92108160 CN92108160 CN 92108160 CN 92108160 A CN92108160 A CN 92108160A CN 1079769 A CN1079769 A CN 1079769A
Authority
CN
China
Prior art keywords
water
heat insulation
heat
powder
waterproofing
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN 92108160
Other languages
English (en)
Inventor
向世伟
李孟春
李光展
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
MIANZHU PHOSPHOROUS FERTILIZER PLANT SICHUAN PROV
Original Assignee
MIANZHU PHOSPHOROUS FERTILIZER PLANT SICHUAN PROV
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by MIANZHU PHOSPHOROUS FERTILIZER PLANT SICHUAN PROV filed Critical MIANZHU PHOSPHOROUS FERTILIZER PLANT SICHUAN PROV
Priority to CN 92108160 priority Critical patent/CN1079769A/zh
Publication of CN1079769A publication Critical patent/CN1079769A/zh
Pending legal-status Critical Current

Abstract

本发明涉及一种建筑用隔热防水粉的生产工艺, 其特征是将一定比例的碳酸钙、憎水剂和水,充分混 合并搅拌成糊状,升温至100℃~250℃,并保温干燥 0.5~3小时即制成隔热防水粉。本工艺生产成本 低,比现有一般防水粉低10~70%,以水为分散介 质,因而生产中无任何污染,产品性能稳定,使用方 便,宜用于建筑业的房屋、管道等的隔热、防水、防渗、 防漏用。

Description

本发明涉及一种建筑用隔热防水材料的制造工艺。
房屋、管道的隔热、防水、防潮是建筑业的一大难题。为解决这一问题,国内近几年来隔热防水材料的研制发展迅速,如CN87101009公开了一种拒水粉,是用Ca(OH)为核心,外包裹由氨水和脂肪酸制成的皂液,再升温干燥而成。又如CN1056513A公开的“隔热镇水粉”,是用石灰石、白云石、大理石微粒为核心,加温后,外表喷射十八酸(或石蜡)封闭而成。上述这些制造工艺各有特点,但工艺都较复杂,生产成本高,有的在加工过程中产出有害物质,污染环境,难以满足用户的需要。
本发明的目的是针对现有各类隔热防水材料制造工艺存在的缺点,提出了一种工艺简单、原料成本低,并具有防水、隔热、绝缘、阻燃等性能良好的、能满足建筑需要的新型隔热防水粉。
本发明的技术方案如下:
将配比为:
过100目的碳酸钙:100
憎水剂:0.2~1.5
水:50~100
上述材料混合并充分搅拌成糊状后,升温至100℃~250℃,经0.5~3小时干燥,使之发生化学物理改性,即得到隔热防水粉。
上述的碳酸钙可为轻质碳酸钙也可为重质碳酸钙。
上述的憎水剂是一种复配物,其配比如下:
石蜡:10~20
十八酸:2~10
三乙醇胺:0.5~5
水:70~80
本发明采用廉价原料制造,可明显地降低成本,比一般防水粉成本低10~70%;以水为分散介质,无任何污染;工艺简单,操作容易,产品性能稳定,无毒无害,使用方便,宜于推广。
以下说明实施例:
先按下列配比:
石蜡:15.6
十八酸:4.6
三乙醇胺:2
水:77.8
配制成憎水剂备用。称取过100目碳酸钙100克,再按下列配比:
碳酸钙:100
憎水剂:0.7
水:80
把上述材料混合并搅拌成糊状防水浆,装入浅盘容器内,加热至200℃,保温2小时后,疏松或过筛后即制成隔热防水粉。
上述隔热防水粉的检测指标如下:
容重:松0.356~紧0.732
防渗性能:1CM厚防水粉在1米水柱静压下19天以上无渗漏。
隔热性能:1CM防水粉隔热温差8℃~10℃。
电绝缘性能:1CM厚防水粉7500伏电压方可击穿。
耐碱性能:1CM厚防水粉在1米水柱的饱和氢氧化钙溶液静压浸泡下八天以上无渗漏。

Claims (3)

1、一种建筑隔热防水粉生产工艺,其特征是将下列配比:
过100目的碳酸钙  100
憎水剂:         0.2~1.5
水:             50~100
的上述材料混合充分并搅拌成糊状,升温至100℃~250℃,经0.5~3小时保温干燥即制成隔热防水粉。
2、根据权利要求1所述的隔热防水粉生产工艺,其特征是憎水剂为一种复配物,其组分配比为:
石蜡:10~20
十八酸:2~10
三乙醇胺:0.5~5
水:70~80
3、根据权利要求1所述的隔热防水粉生产工艺,其特征是碳酸钙可为轻质碳酸钙也可为重质碳酸钙。
CN 92108160 1992-06-08 1992-06-08 建筑隔热防水粉 Pending CN1079769A (zh)