CN104028285A - Cu2ZnSnS4/La2Ti2O7异质结光催化复合材料的制备方法 - Google Patents

Cu2ZnSnS4/La2Ti2O7异质结光催化复合材料的制备方法 Download PDF

Info

Publication number
CN104028285A
CN104028285A CN201410210334.1A CN201410210334A CN104028285A CN 104028285 A CN104028285 A CN 104028285A CN 201410210334 A CN201410210334 A CN 201410210334A CN 104028285 A CN104028285 A CN 104028285A
Authority
CN
China
Prior art keywords
la2ti2o7
czts
preparation
composite material
composite
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201410210334.1A
Other languages
English (en)
Inventor
刘晶冰
田晓萌
严辉
汪浩
朱满康
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Beijing University of Technology
Original Assignee
Beijing University of Technology
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Beijing University of Technology filed Critical Beijing University of Technology
Priority to CN201410210334.1A priority Critical patent/CN104028285A/zh
Publication of CN104028285A publication Critical patent/CN104028285A/zh
Pending legal-status Critical Current

Abstract

Cu2ZnSnS4/La2Ti2O7异质结光催化复合材料的制备方法属于光催化复合材料领域。该复合材料是采用水热法,通过原位生长的过程制备的。首先以La(NO3)3·6H2O和Ti(SO4)2为原料水热法制备出La2Ti2O7纳米片,再将CuCl2、ZnCl2、SnCl2、硫代乙酰胺按2:1:1:8的比例依次加入容有La2Ti2O7的乙二醇中,经过搅拌和超声,转入水热釜高压加热后,得到CZTS/La2Ti2O7复合物。CZTS均匀地分散生长在La2Ti2O7的表面,二者的良好结合有利于光生载流子更好地分离。通过半导体的复合,不但拓展了单一半导体的光响应范围,而且由于不同带隙半导体间光生载流子的输运与分离,抑制了光生电子-空穴对的复合,从而提高了复合半导体催化剂的光催化活性。

Description

Cu2ZnSnS4/La2Ti2O7异质结光催化复合材料的制备方法
技术领域
本发明属于光催化剂技术领域,具体涉及到一种Cu2ZnSnS4(CZTS)/La2Ti2O7异质结光催化复合材料的制备方法。
背景技术
环境和能源已经成为普遍关注的世界性问题,光催化技术及相关材料的开发逐渐成为材料学及催化科学研究的热点。但是单一的光催化剂很难有效地同时吸收紫外光和可见光,并且光生载流子复合几率高,这就限制了其光催化活性。
作为一种具有独特结构和良好活性的层状材料,n型半导体La2Ti2O7在光催化领域得到了广泛的关注。但是La2Ti2O7只能在紫外光下具有光催化活性,而波长在400nm以下的紫外光部分不足太阳光总能量的5%,因此在很大程度上降低了其使用价值。
为提高光催化效率,拓展响应波长范围,将两种或两种以上能带结构匹配的半导体化合物进行复合来构建异质结光催化剂是实现对某一波长有较好光催化效果的有效方法。。
发明内容
本发明的目的在于解决La2Ti2O7光吸收性差和光生载流子复合机率高的问题,而提供了一种CZTS/La2Ti2O7异质结可见光光催化复合材料,同时提供了一种简单有效的制备方法。本发明实现了CZTS/La2Ti2O7异质结光催化复合材料在可见光下良好的光催化性能。
本发明所提供制备方法,包括以下几个步骤:
Cu2ZnSnS4/La2Ti2O7异质结可见光光催化复合材料的制备方法,其特征在于,包括以下步骤:
1)将La(NO3)3·6H2O和Ti(SO4)2按摩尔比为1:1的比例溶于去离子水中,在搅拌条件下加入NaOH,使NaOH浓度为1mol/L;充分搅拌后,将溶液转入带有聚四氟乙烯衬里的高压釜里,在200℃下加热24小时;自然冷却后,产物经水洗,离心分离,在90℃干燥后得 到La2Ti2O7
2)称取La2Ti2O7加入到乙二醇中,搅拌形成悬浮液;La2Ti2O7与Cu2ZnSnS4的摩尔比为1:0.2~0.8;
3)在磁力搅拌下,将CuCl2、ZnCl2、SnCl2、硫代乙酰胺按2:1:1:8的摩尔比依次加入上述悬浮液中;
4)将经过步骤3)后得到的悬浮液超声30min后,转移到水热釜中里,180℃下加热15个小时;自然冷却后,反复洗涤、离心分离,在90℃干燥后得CZTS/La2Ti2O7复合物。
本发明采用原位生长的方法制备了CZTS/La2Ti2O7异质结可见光光催化复合材料,CZTS均匀地分散生长在La2Ti2O7的表面,二者的良好结合有利于光生载流子更好地分离。由于La2Ti2O7是宽带隙的n-型半导体,而CZTS是窄带隙的p-型半导体材料,且光吸收系数很高(>104cm-1),通过半导体的复合,不仅拓展了复合材料的光响应范围,而且由于不同带隙半导体间光生载流子的输运与分离,抑制了光生电子-空穴对的复合,从而提高了复合半导体催化剂的光催化活性。
附图说明
图1为本发明实施例1、实施例2和实施例3产物的XRD图。
图2为本发明实施例2产物的扫描电镜照片。
具体实施方式
下面结合附图和具体实施方式,进一步阐明本发明的实质性特点和显著优点,本发明决非仅局限于所陈述的实施例。
实施例1
1)将2.165g La(NO3)3·6H2O和1.200g Ti(SO4)2依次溶于去离子水中,在搅拌条件下加入NaOH,使NaOH的浓度为1mol/L。充分搅拌后,将溶液转入带有聚四氟乙烯衬里的高压釜里,在200℃下加热24小时。自然冷却后,产物经水洗,离心分离,在90℃干燥后得到La2Ti2O7
2)称取0.4g La2Ti2O7加入到40mL乙二醇中,搅拌形成悬浮液。
3)在磁力搅拌下,将0.0627g CuCl2、0.0251ZnCl2、0.0415gSnCl2、0.1106g硫代乙酰胺依次加入悬浮液中。
4)将悬浮液超声30min后,转移到50mL的水热釜中里,180℃下加热15个小时。自然冷却后,反复洗涤、离心分离,在90℃干燥后得CZTS/La2Ti2O7复合物。
由图1中的b可以看出由于CZTS含量较少,且与La2Ti2O7的峰有重合的地方,所以几乎看不到CZTS的衍射峰。图1中的a是纯La2Ti2O7XRD图。图1中的e是纯Cu2ZnSnS4XRD图。
表1为60min内此复合材料的可见光催化降解效率。
表1
反应时间/min 0 10 20 30 40 50 60
降解效率/% 0 37.1 46.8 51.3 59.5 60.1 65.6
实施例2
1)将2.165g La(NO3)3·6H2O和1.200g Ti(SO4)2依次溶于去离子水中,在搅拌条件下加入NaOH,使NaOH的浓度为1mol/L。充分搅拌后,将溶液转入带有聚四氟乙烯衬里的高压釜里,在200℃下加热24小时。自然冷却后,产物经水洗,离心分离,在90℃干燥后得到La2Ti2O7
2)称取0.4g La2Ti2O7加入到40mL乙二醇中,搅拌形成悬浮液。
3)在磁力搅拌下,将0.1568g CuCl2、0.0627ZnCl2、0.1038gSnCl2、0.2765g硫代乙酰胺依次加入悬浮液中,保证每一步得到的是澄清溶液。
4)将悬浮液超声30min后,转移到50mL的水热釜中里,180℃下加热15个小时。自然冷却后,反复洗涤、离心分离,在90℃干燥后得CZTS/La2Ti2O7复合物。
由图1中的c可以看出La2Ti2O7中出现CZTS的衍射峰。由图2看出CZTS均匀生长在La2Ti2O7纳米片上。表2为60min内此复合材料的可 见光催化降解效率。
表2
反应时间/min 0 10 20 30 40 50 60
降解效率/% 0 46.7 52.8 57.8 65.0 69.2 73.8
实施例3
1)将2.165g La(NO3)3·6H2O和1.200g Ti(SO4)2依次溶于去离子水中,在搅拌条件下加入NaOH,使NaOH的浓度为1mol/L。充分搅拌后,将溶液转入带有聚四氟乙烯衬里的高压釜里,在200℃下加热24小时。自然冷却后,产物经水洗,离心分离,在90℃干燥后得到La2Ti2O7
2)称取0.4g La2Ti2O7加入到40mL乙二醇中,搅拌形成悬浮液。
3)在磁力搅拌下,将0.2509g CuCl2、0.1003ZnCl2、0.1661gSnCl2、0.4424g硫代乙酰胺依次加入悬浮液中,保证每一步得到的是澄清溶液。
4)将悬浮液超声30min后,转移到50mL的水热釜中里,180℃下加热15个小时。自然冷却后,反复洗涤、离心分离,在90℃干燥后得CZTS/La2Ti2O7复合物。
由图1中的d可以看出La2Ti2O7中CZTS的衍射峰更加明显。表3为此60min内复合材料的可见光催化降解效率
表3
反应时间/min 0 10 20 30 40 50 60
降解效率/% 0 32.6 44.7 50.1 57.3 60.0 66.7

Claims (1)

1.Cu2ZnSnS4/La2Ti2O7异质结光催化复合材料的制备方法,其特征在于,包括以下步骤:
1).将La(NO3)3·6H2O和Ti(SO4)2按摩尔比为1:1的比例溶于去离子水中,在搅拌条件下加入NaOH,使NaOH浓度为1mol/L;充分搅拌后,将溶液转入带有聚四氟乙烯衬里的高压釜里,在200℃下加热24小时;自然冷却后,产物经水洗,离心分离,在90℃干燥后得到La2Ti2O7
2).称取La2Ti2O7加入到乙二醇中,搅拌形成悬浮液;La2Ti2O7与Cu2ZnSnS4的摩尔比为1:0.2~0.8;
3).在磁力搅拌下,将CuCl2、ZnCl2、SnCl2、硫代乙酰胺按2:1:1:8的摩尔比依次加入上述悬浮液中;
4).将悬浮液超声30min后,转移到水热釜中里,180℃下加热15个小时;自然冷却后,反复洗涤、离心分离,在90℃干燥后得CZTS/La2Ti2O7复合物。
CN201410210334.1A 2014-05-17 2014-05-17 Cu2ZnSnS4/La2Ti2O7异质结光催化复合材料的制备方法 Pending CN104028285A (zh)