CN1257951A - Polyester staple fiber spinning oil and manufacturing method thereof - Google Patents

Polyester staple fiber spinning oil and manufacturing method thereof Download PDF

Info

Publication number
CN1257951A
CN1257951A CN 99124281 CN99124281A CN1257951A CN 1257951 A CN1257951 A CN 1257951A CN 99124281 CN99124281 CN 99124281 CN 99124281 A CN99124281 A CN 99124281A CN 1257951 A CN1257951 A CN 1257951A
Authority
CN
China
Prior art keywords
spinning oil
agent
phosphate
antistatic additive
oil
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN 99124281
Other languages
Chinese (zh)
Inventor
王伟松
王新荣
杨树良
金一丰
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Zhejiang Huangma Chemical Industry Group Co ltd
Original Assignee
Zhejiang Huangma Chemical Industry Group Co ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Zhejiang Huangma Chemical Industry Group Co ltd filed Critical Zhejiang Huangma Chemical Industry Group Co ltd
Priority to CN 99124281 priority Critical patent/CN1257951A/en
Publication of CN1257951A publication Critical patent/CN1257951A/en
Pending legal-status Critical Current

Abstract

A polyester staple fiber spinning oil agent and a manufacturing method thereof are disclosed, wherein the weight percentage of each component is 10-20% of a smoothing agent, 5-15% of a bundling agent and 70-80% of an antistatic agent.

Description

Spinning oil for terylene staple and manufacture method thereof
The present invention relates to a kind of spinning oil for terylene staple and manufacture method thereof, belong to the auxiliary agent manufacturing technology field in the synthetic fiber process technology.
Will pass through spinning when polyester staple fiber is produced in the chemical fibre factory, drawing-off is curled, and operations such as cut-out add man-hour again through operations such as blowing, comb and parallel cotton fibers prior to spinning, drafting, rove, spun yarns behind the cotton mill.All there is friction between fiber and fiber, fiber and metallic weapon between each procedure and produces a large amount of electrostatic charges, and along with the quickening electrostatic problem of draw speed is more outstanding, thereby to the antistatic behaviour of short-staple Dacron oil solution, overall balance requires very high between flatness and the convergence.
The purpose of this invention is to provide a kind of stable performance, good spinnability can satisfy the polyester staple fiber spinning process requirement, effectively improves the short-staple Dacron oil solution and the manufacture method thereof of polyester staple fiber spinning quality.
The present invention is a spinning oil for terylene staple, mainly by smooth agent, and collecting agent, compositions such as antistatic additive is characterized in that the percentage by weight of each component is: smooth agent 10~20%, collecting agent 5~15%, antistatic additive 70~80%,
Described smooth agent can be mineral oil, double base alcohol ester, triol ester, quaternary alcohol ester, the mixture of one or more in the high molecular weight polyether.The effect of smooth agent can keep between fiber and the fiber, the suitable coefficient of friction between fiber and other contact components, improves level and smooth performance, helps carrying out smoothly of spin-drawing.
Described collecting agent can be the polyethylene glycol Glycol Oleic Acid Ester, aliphatic acid polyethenoxy ether, polyethylene glycol laurate dibasic acid esters, castor oil polyoxyethylene ether, the mixture of one or more in the octanol high-molecular weight atactic polyethers.The adding of collecting agent can improve the convergence of finish, makes fiber not fluffy, at random in process, and fiber is played the obvolvent effect.
Described antistatic additive can be lauryl alcohol phosphate polyoxyethylene ether sylvite, hexadecanol phosphate kalium salt, octadecanol phosphate kalium salt, lauryl alcohol polyoxyethylene ether phosphate sylvite, the mixture of one or more in the amphoteric phosphate ammonium salt.The effect of antistatic additive is can be adsorbed on fiber surface in the high speed spinning process, increases the hygroscopicity of fiber, improves electric conductivity, reduces the accumulation of static.
The manufacture method of spinning oil for terylene staple of the present invention is: the percentage by weight of pressing each component, elder generation is with the antistatic additive suction reactor of accurate measurement, being heated to 40-80 ℃ stirs, with in the collecting agent suction reactor, after stirring, add smooth agent again, after stirring 30-50min, cooling is filtered, packing.
The present invention compared with prior art has following distinguishing feature and good effect:
1, has good antistatic effect, can reduce interfibrous friction, guarantee that terylene front and back procedure carries out smoothly;
2, have good coherent and opening character, feel is abundant;
3, have good flatness, can reduce the card nailing neps in the wool top production, the generation of workprint improves the fiber feel greatly, improves fiber quality;
4, good with the fiber affinity, fuel consumption is low;
Spinning oil for terylene staple of the present invention is applicable to each end production process such as spinning, drawing-off, wool top processing and back processing of polyester staple fiber, uses through the Duo Jia chemical fibre factory, and spinning, the production that stretches run well, and the fiber quality index reaches customer requirements.
Below in conjunction with embodiment the present invention is further described:
By weight percentage, determine the ratio of each component:
Embodiment 1:
Collecting agent 10%, wherein aliphatic acid polyethenoxy ether (LAE-9 class) 2%, octanol high-molecular weight atactic polyethers 8%;
Antistatic additive 75%, wherein hexadecanol phosphate kalium salt (PK class) 45%, amphoteric phosphate ammonium salt 30%;
Smooth agent 15% is high molecular weight polyether.
Embodiment 2:
Collecting agent 12%, wherein the polyethylene glycol Glycol Oleic Acid Ester 5%, castor oil polyoxyethylene ether (EL class) 7%;
Antistatic additive 72%, lauryl alcohol phosphate polyoxyethylene ether sylvite (EP class) 50% wherein, lauryl alcohol polyoxyethylene phosphate sylvite (MPK class) 22%;
Smooth agent 16%, wherein triol ester 4%, high molecular weight polyether 10%, mineral oil 2%.
Embodiment 3:
Collecting agent 9%, polyethylene glycol laurate dibasic acid esters 5% wherein, aliphatic acid polyethenoxy ether (LAE-9 class) 4%;
Antistatic additive 78%, octadecanol phosphate kalium salt (PK class) 54% wherein, lauryl alcohol polyoxyethylene ether phosphate sylvite 24%;
Smooth agent 13%, wherein binary alcohol esters 30%, end capped polyether 15%, polybutene class 16%.
After the described ratio batching of above-mentioned three embodiment, the manufacture method of its spinning oil for terylene staple is:
With antistatic additive suction reactor, open and stir earlier, be warming up to about 50 ℃, stir, with collecting agent suction reactor, stir again, add smooth agent at last, keep about 50 ℃ of temperature, stir 30min, stir and finish, be cooled to about 40 ℃, blowing, filtration, packing are promptly.
The spinning oil for terylene staple of producing according to proportioning of the present invention and manufacture method can reach following quality index:
1, the white lotion of outward appearance (25 ℃)
2, pH value (10% aqueous solution, 20 ℃) 6.0-8.0
3, effective component content (%, 〉=) 30.0
4, stable one week of 2% aqueous solution is not stratified

Claims (5)

1, a kind of spinning oil for terylene staple, by flatness, collecting agent, antistatic additive is formed, and it is characterized in that the percentage by weight of each component is: smooth agent 10~20%, collecting agent 5~15%, antistatic additive 70~80%.
2, by the described spinning oil for terylene staple of claim 1, it is characterized in that described smooth agent can be mineral oil, double base alcohol ester, triol ester, quaternary alcohol ester, the mixture of one or more of high molecular weight polyether.
3, by the described spinning oil for terylene staple of claim 1, it is characterized in that described collecting agent can be the polyethylene glycol Glycol Oleic Acid Ester, aliphatic acid polyethenoxy ether, polyethylene glycol laurate dibasic acid esters, castor oil polyoxyethylene ether, the mixture of one or more in the octanol high-molecular weight atactic polyethers.
4, by the described spinning oil for terylene staple of claim 1, it is characterized in that described antistatic additive can be lauryl alcohol phosphate polyoxyethylene ether sylvite, the hexadecanol phosphate kalium salt, the octadecanol phosphate kalium salt, lauryl alcohol polyoxyethylene ether phosphate sylvite, the mixture of one or more in the amphoteric phosphate ammonium salt.
5, by claim 1 or 2,3, the manufacture method of 4 described spinning oil for terylene staple, it is characterized in that percentage by weight by each component, with the antistatic additive suction reactor of accurate measurement, be heated to 40~80 ℃ and stir, earlier again with in the collecting agent suction reactor, after stirring, add smooth agent, behind the stirring 30-50min, cooling, filter packing.
CN 99124281 1999-12-21 1999-12-21 Polyester staple fiber spinning oil and manufacturing method thereof Pending CN1257951A (en)