JP2002038032A - 熱可塑性プラスチックの抗菌防カビ組成物 - Google Patents

熱可塑性プラスチックの抗菌防カビ組成物

Info

Publication number
JP2002038032A
JP2002038032A JP2000258161A JP2000258161A JP2002038032A JP 2002038032 A JP2002038032 A JP 2002038032A JP 2000258161 A JP2000258161 A JP 2000258161A JP 2000258161 A JP2000258161 A JP 2000258161A JP 2002038032 A JP2002038032 A JP 2002038032A
Authority
JP
Japan
Prior art keywords
antibacterial
resin
thermoplastic
composition
polyhexamethylene guanidine
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP2000258161A
Other languages
English (en)
Inventor
Tomiyoshi Suyama
富義 陶山
Takahiro Muramatsu
高広 村松
Won Son Son
ウォン ソン ソン
Hon Shin Ju
ホン シン ジュ
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
SK CORP
Daiwa Chemical Industries Ltd
Original Assignee
SK CORP
Daiwa Chemical Industries Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by SK CORP, Daiwa Chemical Industries Ltd filed Critical SK CORP
Priority to JP2000258161A priority Critical patent/JP2002038032A/ja
Publication of JP2002038032A publication Critical patent/JP2002038032A/ja
Pending legal-status Critical Current

Abstract

(57)【要約】 【目的】 プラスチック練り込み用抗菌防カビ剤として
練り込み時の温度にも分解せず、しかもプラスチックの
物性に全く影響を与えることのない優れた抗菌防カビ剤
である。 【構成】 ポリヘキサメチレングアニジン塩をプラスチ
ックに直接、あるいはマスターバッチとしたものを練り
込み、半永久的な抗菌防カビ性を付与するものである。

Description

【発明の詳細な説明】
【0001】
【発明の属する技術分野】本発明は、熱可塑性プラスチ
ックに抗菌防カビ組成物としてポリヘキサメチレングア
ニジン塩を練り込み、長期間抗菌防カビ効力を持続させ
る抗菌防カビ組成物に関する。詳しくは、ポリヘキサメ
チレングアニジン塩をそのまま、あるいはそれのマスタ
ーバッチを直接熱可塑性プラスチックに練り込み、フィ
ルム、フィラメント、成型物等に半永久的に抗菌防カビ
効果を持続させる組成物である。
【0002】
【従来の技術】プラスチックのフィルム、フィラメント
や成型物に対する抗菌防カビ剤の処理方法は、抗菌防カ
ビ組成物を直接プラスチックの表面に加工する方法が一
般的であった。しかし、このような方法では水洗や表面
の摩擦等で薬剤が脱落しやすく、長期間効果を持続する
ことが困難であった。恒久的に抗菌防カビ性を付与する
方法として、素材であるプラスチックに練り込むことが
考えられる。
【0003】しかしながら、熱可塑性プラスチックに練
り込むを行なうことは、抗菌防カビ組成物にプラスチッ
クの加工温度よりも高い耐熱性が必要となる。耐熱性の
低い抗菌防カビ組成物を熱可塑性プラスチックに練り込
んでしまうと、プラスチックの着色、抗菌防カビ効果の
低下、あるいはプラスチックの物性低下等実用に即さな
い結果となってしまう。このようなことから、熱に対し
て安定な銀、亜鉛等の金属イオンを含む種々の化合物が
応用されているのが従来の方法である。
【0004】
【発明が解決しようとする課題】プラスチックへの抗菌
防カビ加工として、プラスチックの表面加工はプラスチ
ックと薬剤の親和性、浸透性が悪い為、たとえ表面に処
理しても長期間の効果を期待することができない。抗菌
防カビ剤をプラスチックの加工時に練り込むことは、抗
菌防カビ組成物の耐熱性の問題及びプラスチックとの相
溶性や物性の変化が障害となって思うような進展が見ら
れなかった。
【0005】本発明は、以上のような欠点がなくプラス
チックに溶融状態で練り込みを行なっても分解、変色あ
るいはプラスチックに悪影響を与えることが少ない化合
物で、しかも抗菌防カビ性に優れた化合物の実用化試験
を行ない、充分に効果の見られる化合物の開発を行なっ
た。一般に有機化合物は酸素、紫外線及び熱に対して影
響を受けやすい物質が多い。特に熱に対しては特定な化
合物を除いて分解、変色するものが多い。
【0006】抗菌防カビ性を有する有機化合物を構造的
にみると脂肪族系、芳香族系を問わず窒素、硫黄、ハロ
ゲンを含有する化合物や二重結合、三重結合を持った不
飽和化合物の他エステル、アルデヒド、フェノール系化
合物あるいは複素環式化合物等は物質の差はあるものの
酸化、還元の影響を受けやすいものである。本発明は、
以上のような欠点の少ない安定した化合物で、しかも抗
菌防カビ効果に優れた化合物の発見のために研究を行な
った。
【0007】
【課題を解決するための手段】プラスチックを加工する
際の溶融状態で抗菌防カビ組成物を練り込むためには、
その温度に対する安定性とプラスチックに均一に相溶配
合され、しかもその化合物がプラスチックフィルムや成
型品の表面に於いて抗菌防カビ効力が発揮されなければ
ならない。ポリヘキサメチレングアニジン塩は優れた抗
菌防カビ組成物として使用されている安全性の高く、環
境に優しい抗菌防カビ剤である。
【0008】プラスチックは、用途、目的に応じて素材
を選択することができる。使用する熱可塑性プラスチッ
クとしては、ポリエチレン樹脂、ポリプロピレン樹脂、
ポリウレタン樹脂、ポリアクリル樹脂、ポリアミド樹
脂、ポリスチレン樹脂、ポリ塩化ビニル樹脂、ABS樹
脂、ポリエステル樹脂等で、それらの成型品、フィル
ム、繊維製品等に応用することができる。また用途別で
は、工業用をはじめ家庭用電化製品、キッチンや浴室用
等の日用雑貨品類、衣料品、天幕、包装用フィルム、農
業用フィルム、漁業用の漁網やロープからOA機器、コ
ンピューター関係の精密電化製品のほか各種産業用に広
く応用することができる。
【0009】プラスチックに対するポリヘキサメチレン
グアニジン塩の添加量は、0.05〜5.0重量%(以
下総て重量%で示す)好ましくは0.1〜2.0%をそ
のままかあるいはマスターバッチとして添加する。
【0010】本発明には、この他に他の殺菌剤、防カビ
剤、防虫剤、消臭剤及びこれらに対する効力増強剤の使
用や着香剤、着色剤、紫外線防止剤、酸化防止剤を併用
することができる。また、プラスチックへの練り込みに
際して各種可塑剤、酸化亜鉛、炭酸カルシウム、シリカ
その他の微粉天然鉱物質等を使用することができる。
【0011】以下、実施例により詳細説明する。しか
し、本発明はこれらの実施例に限定されるものではな
い。
【0012】
【実施例】(実験例1)ポリヘキサメチレングアニジン
リン酸塩をポリエチレンペレットに1.0%,0.5
%,0.3%,0.1%をそれぞれ添加した後、二軸押
出し機(PCM30(株)池貝)により温度150〜1
70℃にてコンパウンド化した後、射出成型機(SVH
−30−50−P:(株)山城精機製作所)にてプレー
トを試作した。抗菌防カビ試験結果は、表1に示す。
【0013】抗菌防カビ試験方法 このプレートに対する抗菌防カビ試験は、次に示す方法
で行った。
【0014】 抗菌試験・・・JIS L−1902 ハロー法による。 供試細菌 Staphylococcus aureus ATCC 6538P(黄色ブドウ球菌) Escherichia coli IFO 3972( 大腸菌) 判定方法 試料の周囲にできた阻止帯のあるものは、あり、無いもの は、なし、とする。
【0015】 防カビ試験・・JIS Z−2911による。 供試カビ Aspergillus niger FERM S−1 Penicillium citrinum FERM S−5 Cladosporium cladosporioid es FERM S−8 判定方法 次の表に示す表示方法による。 カビ抵抗性表示 カビの発育 3 試料に接種したカビの発育が認められない。 2 試料に接種したカビの発育面積が1/3を超えない。 1 試料に接種したカビの発育面積が1/3を超える。 (註)この表示方法において、表示3でさらに試料の周囲に阻止帯がある 場合には、その阻止帯の大きさをmm数で右側に表示する。
【0016】(実験例2)ポリヘキサメチレングアニジ
ン硫酸塩をポリスチレンペレットに1.0%,0.5
%,0.3%,0.1%をそれぞれ添加した後、温度2
30〜250℃にてコンパウンド化した後、プレートを
試作した。抗菌防カビ試験結果は、表2に示す。
【0017】(実験例3)ポリヘキサメチレングアニジ
ン酢酸塩を熱可塑性ウレタン樹脂に1.0%,0.5
%,0.3%,0.1%をそれぞれ添加した後コンパウ
ンド化し、プレートを試作した。抗菌防カビ試験結果
は、表3に示す。
【0018】(実験例4)ポリヘキサメチレングアニジ
ンリン酸塩を塩化ビニル樹脂(DOP 40%)に1.
0%,0.5%,0.3%,0.1%をそれぞれ添加し
た後コンパウンド化し、プレートを試作した。抗菌防カ
ビ試験結果は、表4に示す。
【0019】
【表1】
【0020】
【表2】
【0021】
【表3】
【0022】
【表4】
【0023】
【発明の効果】本発明化合物であるポリヘキサメチレン
グアニジン塩は、プラスチック練り込みを行っても分
解、着色がなく、充分に耐えられる性質を有している。
しかも、プラスチックへの着色や物性を全く損なうこと
なく、半永久的な抗菌防カビ性を付与する組成物として
使用できる優れたものである。しかも低毒性であるので
工業用、OA機器用、家庭用、漁業用、農業用と広く一
般のプラスチック製品の抗菌防カビ組成物として安心し
て応用することができる。
───────────────────────────────────────────────────── フロントページの続き (72)発明者 村松 高広 東京都江戸川区中央4丁目17番28号 大和 化学工業株式会社内 (72)発明者 ソン ウォン ソン 大韓民国デジョン市ユソング、ジョンミン ドン462−5 セゾンアパート (72)発明者 ジュ ホン シン 大韓民国デジョン市ユソング、ジョンミン ドン462−5 セゾンアパート Fターム(参考) 4F070 AA13 AA15 AA18 AA19 AA32 AA47 AA53 AA54 AC45 FA03 FC05 4H011 AA02 AA03 BA01 BB11 BC19 DH02 DH04 DH05 4J002 BB031 BB121 BC031 BD031 BG021 BN151 CF001 CK001 CL001 ER026 FD186

Claims (4)

    【特許請求の範囲】
  1. 【請求項1】 熱可塑性プラスチックに抗菌防カビ組成
    物としてポリヘキサメチレングアニジン塩をプラスチッ
    クの溶融時に練り込むことを特徴とする熱可塑性プラス
    チックの抗菌防カビ組成物。
  2. 【請求項2】 熱可塑性プラスチックとして、ポリエチ
    レン樹脂、ポリプロピレン樹脂、ポリウレタン樹脂、ポ
    リアクリル樹脂、ポリアミド樹脂、ポリスチレン樹脂、
    ポリ塩化ビニル樹脂、ABS樹脂、ポリエステル樹脂に
    150〜300℃の温度で抗菌防カビ組成物としてポリ
    ヘキサメチレングアニジン塩を練り込むことを特徴とす
    る請求項1記載の熱可塑性プラスチックの抗菌防カビ組
    成物。
  3. 【請求項3】 熱可塑性プラスチックの抗菌防カビ組成
    物としてポリヘキサメチレングアニジン塩を0.01〜
    10.0重量%を溶融時のプラスチックに練り込むこと
    を特徴とする請求項1〜2記載の熱可塑性プラスチック
    の抗菌防カビ組成物。
  4. 【請求項4】 ポリヘキサメチレングアニジン塩の塩類
    は、塩酸,硫酸,リン酸,硝酸等の無機塩の他、有機酸
    の塩でもよい。
JP2000258161A 2000-07-26 2000-07-26 熱可塑性プラスチックの抗菌防カビ組成物 Pending JP2002038032A (ja)