CN103882756A - 高速宽幅生活用纸专用成形网 - Google Patents

高速宽幅生活用纸专用成形网 Download PDF

Info

Publication number
CN103882756A
CN103882756A CN201410130387.2A CN201410130387A CN103882756A CN 103882756 A CN103882756 A CN 103882756A CN 201410130387 A CN201410130387 A CN 201410130387A CN 103882756 A CN103882756 A CN 103882756A
Authority
CN
China
Prior art keywords
paper
parallel
layer
daily use
polyester
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201410130387.2A
Other languages
English (en)
Inventor
陆平
周积学
叶平
盛长新
孙勇
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
JIANGSU JINNI ENGINEERING FABRIC Co Ltd
Original Assignee
JIANGSU JINNI ENGINEERING FABRIC Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by JIANGSU JINNI ENGINEERING FABRIC Co Ltd filed Critical JIANGSU JINNI ENGINEERING FABRIC Co Ltd
Priority to CN201410130387.2A priority Critical patent/CN103882756A/zh
Publication of CN103882756A publication Critical patent/CN103882756A/zh
Pending legal-status Critical Current

Abstract

本发明公开了一种高速宽幅生活用纸专用成形网,为采用20片综框将聚酯或尼龙单丝交织而成的整体复合交织物,包括成纸层、中间连接层和机器层三层不同的织造结构,其最小组织单元由20根聚酯单丝作为经线和40根聚酯或尼龙单丝作为纬线构成,其中所述成纸层采用5综缎纹编织法,所述机器层采用5综缎纹编织织法,所述中间连接层包括一对缝合纬线,将成纸层与机器层连接起来。本发明中由于成纸层采用5综缎纹编织法,使成形网纤维支撑指数提高,生活用纸的纤维和填料留着率提高,纸页成形均匀,纸页易从网上剥离,成纸更平整细腻。上下层结合更加牢固。机器层采用5综缎纹编织织法,使成形网的耐磨性得到了提高,使用寿命更长。

Description

高速宽幅生活用纸专用成形网
技术领域
本发明涉及一种高速宽幅生活用纸专用成形网,具体讲是一种应用在生产生活用纸造纸机的湿部,起纸页成形、脱水和传送作用的一种脱水器材。
背景技术
造纸成形网是造纸机湿部重要的成形和脱水材料,高速宽幅生活用纸造纸机对成形网有着特殊的要求。高速宽幅生活用纸的造纸机网案短,要求成形网脱水快;同时因为生活用纸纸页薄、克重低,要求成形网纤维支撑指数高、成纸无网痕;另外要求生产的生活用纸柔软、蓬松。
现有的造纸成形网仅能在低车速生活用纸造纸机上使用,虽然基本能完成纸页成形和脱水任务,但其不足之处是现有的造纸成形网成纸面纤维支撑指数不高,造成生活用纸成品表面网痕明显、生活用纸的纤维和填料留着率低,而且现有的造纸成形网脱水能力差,不适应高车速生活用纸造纸机的需要。
发明内容
为克服现有技术的不足,本发明提供了一种高速宽幅生活用纸专用成形网,其成纸面平整,使用寿命长,脱水能力强,完全能适应高速生活用纸纸机需要。
本发明采取的技术方案为:一种高速宽幅生活用纸专用成形网,为采用20片综框将聚酯或尼龙单丝交织而成的整体复合交织物,包括成纸层、中间连接层和机器层三层不同的织造结构,其最小组织单元由20根聚酯单丝作为经线和40根聚酯或尼龙单丝作为纬线构成,其中所述成纸层采用5综缎纹编织法,所述机器层采用5综缎纹编织织法,所述中间连接层包括一对缝合纬线,一对缝合纬线与成纸层的经线及机器层的经线交织,将成纸层与机器层缝合起来。
作为本发明优选的技术方案,所述成纸层与机器层的经线根数比为1:1。
作为本发明优选的技术方案,所述成纸层与机器层的纬线根数比为2:1。
作为本发明优选的技术方案,所述中间连接层的纬线根数占总纬线根数的1/2。
作为本发明优选的技术方案,所述成纸层中,经线直径为0.12-0.15mm,纬线直径为0.11-0.15mm,材料均采用聚酯单丝;机器层中,经线采用聚酯单丝,经线直径为0.18-0.21mm,纬线直径为0.22-0.27mm ,纬线采用全聚酯单丝;中间连接层中的缝合纬线直径为0.11-0.15mm,材料采用全聚酯单丝或全尼龙单丝;所述高速宽幅生活用纸专用成形网经线密度为60-68根/cm、纬线密度为75-85根/cm。
本发明的有益效果:由于成纸层采用5综缎纹编织法,使高速宽幅生活用纸专用成形网的纤维支撑指数提高,网孔均匀、网面平滑,生活用纸的纤维和填料留着率提高,纸页成形均匀,纸页易从网上剥离,成纸更平整细腻;用一对缝合纬线将这两层连接在一起,上下层结合更加牢固。机器层采用5-综缎纹编织织法,使成形网的耐磨性得到了提高,稳定性得到加强,使用寿命更长,能适应1500-2000米/分钟高速卫生纸造纸机的需要。
附图说明
图1为本发明的最小组织单元织造网纹图,由20根聚酯单丝作为经线,40根聚酯或尼龙单丝作为纬线,白色代表纬线在经线下面,黑色代表和灰色代表代表纬线在经线上面,从上往下4根一循环,第1根是成纸层纬线,第2根是机器层纬线,第3和第4根是中间连接层纬线。
图2-图5为本发明20根经线和40根纬线,经纬分步织造关系图,图中的黑点代表20根经线的横截面,图中的折线代表纬线,并标明40根纬线的编号。
图2为20根经线和第1-12根纬线的经纬分步织造关系图。
图3为20根经线和第13-24根纬线的经纬分步织造关系图。
图4为20根经线和第25-36根纬线的经纬分步织造关系图。
图5为20根经线和第37-40根纬线的经纬分步织造关系图。
下面结合附图对本发明的具体实施方式做进一步阐明。
具体实施方式
实施例1
如图1-5所示,本高速宽幅生活用纸专用成形网是采用20片棕框将聚酯或尼龙单丝交织成成纸层、中间连接层和机器层三层不同织造结构连接成整体的复合交织物,其最小组织单元由20根聚酯单丝作为经线和40根聚酯或尼龙单丝作为纬线构成,其中成纸层和机器层的经线根数比为1:1;纬线根数比2:1;中间连接层的纬线根数占总纬线数的1/2;成纸层采用5综缎纹编织法编织,经线采用聚酯单丝,经线直径为0.12,纬线采用聚酯单丝,纬线直径为0.11,可以增加透气度,提高成形网的脱水能力;同时中间连接层中的缝合纬线与成纸层中的经线交织对成纸面起支撑作用,又与机器层经线交织,起缝合成纸层与机器层的作用,缝合纬线直径为0.11,采用全聚酯或全尼龙单丝;机器层采用5综缎纹编织织法,经线采用聚酯单丝,经线直径为0.18,纬线采用全聚酯单丝,纬线直径为0.22。本高速宽幅生活用纸专用成形网的成品经线密度为68根/cm、纬线密度为85根/cm。
实施例1成形网的测量数据:
Figure 215786DEST_PATH_IMAGE002
实施例2
如图1-5所示,本高速宽幅生活用纸专用成形网是采用20片棕框将聚酯或尼龙单丝交织成成纸层、中间连接层和机器层三层不同织造结构连接成整体的复合交织物,其最小组织单元由20根聚酯单丝作为经线和40根聚酯或尼龙单丝作为纬线构成,其中成纸层和机器层的经线根数比为1:1;纬线根数比2:1;中间连接层的纬线根数占总纬线数的1/2;成纸层采用5综缎纹编织法编织,经线采用聚酯单丝,经线直径为0.15mm,纬线采用聚酯单丝,纬线直径为0.15mm,可以增加透气度,提高成形网的脱水能力;同时中间连接层中的缝合纬线与成纸层中的经线交织对成纸面起支撑作用,又与机器层经线交织,起缝合成纸层与机器层的作用,缝合纬线直径为0.15mm,采用全聚酯或全尼龙单丝;机器层采用5综缎纹编织织法,经线采用聚酯单丝,经线直径为0.21mm,纬线采用全聚酯单丝,纬线直径为0.30mm。本高速宽幅生活用纸专用成形网的成品经线密度为60根/cm、纬线密度为75根/cm。
实施例2成形网的测量数据:
Figure 195243DEST_PATH_IMAGE004
  实施例3
如图1-5所示,本高速宽幅生活用纸专用成形网是采用20片棕框将聚酯或尼龙单丝交织成成纸层、中间连接层和机器层三层不同织造结构连接成整体的复合交织物,其最小组织单元由20根聚酯单丝作为经线和40根聚酯或尼龙单丝作为纬线构成,其中成纸层和机器层的经线根数比为1:1;纬线根数比2:1;中间连接层的纬线根数占总纬线数的1/2;成纸层采用5综缎纹编织法编织,经线采用聚酯单丝,经线直径为0.14mm,纬线采用聚酯单丝,纬线直径为0.13mm,可以增加透气度,提高成形网的脱水能力;同时中间连接层中的缝合纬线与成纸层中的经线交织对成纸面起支撑作用,又与机器层经线交织,起缝合成纸层与机器层的作用,缝合纬线直径为0.13mm,采用全聚酯或全尼龙单丝;机器层采用5综缎纹编织织法,经线采用聚酯单丝,经线直径为0.20mm,纬线采用全聚酯单丝,纬线直径为0.26mm。本高速宽幅生活用纸专用成形网的成品经线密度为63根/cm、纬密为80根/cm。
实施例3成形网的测量数据:
Figure 974981DEST_PATH_IMAGE006
以上数据中成形网厚度的单位为mm。以上数据的测量和计算完全采用了GB/T 24290-2009《造纸成形网、干燥网测量方法》中的方法。其中纤维支撑指数较高,支撑点增多,说明本高速宽幅生活用纸专用成形网对纸的纤维和填料留着率提高,成纸表面网痕大大减少,纸页成形更均匀;脱水指数较高,透气量增加,说明本高速宽幅生活用纸专用成形网对纸的脱水能力提高;成形网厚度和机器层纬线直径的增加,说明本高速宽幅生活用纸专用成形网的耐磨性增加,在纸机上的使用寿命延长。

Claims (5)

1.一种高速宽幅生活用纸专用成形网,为采用20片综框将聚酯或尼龙单丝交织而成的整体复合交织物,包括成纸层、中间连接层和机器层三层不同的织造结构,其最小组织单元由20根聚酯单丝作为经线和40根聚酯或尼龙单丝作为纬线构成,其中所述成纸层采用5综缎纹编织法,所述机器层采用5综缎纹编织织法,所述中间连接层包括一对缝合纬线,一对缝合纬线与成纸层的经线及机器层的经线交织,将成纸层与机器层缝合起来。
2.根据权利要求1所述的高速宽幅生活用纸专用成形网,其特征在于:所述成纸层与机器层的经线根数比为1:1。
3.根据权利要求2所述的高速宽幅生活用纸专用成形网,其特征在于:所述成纸层与机器层的纬线根数比为2:1。
4.根据权利要求3所述的高速宽幅生活用纸专用成形网,其特征在于:所述中间连接层的纬线根数占总纬线根数的1/2。
5.根据权利要求1所述的高速宽幅生活用纸专用成形网,其特征在于:所述成纸层中,经线直径为0.12-0.15mm,纬线直径为0.11-0.15mm,材料均采用聚酯单丝;机器层中,经线采用聚酯单丝,经线直径为0.18-0.21mm,纬线直径为0.22-0.27mm ,纬线采用聚酯单丝;中间连接层中的缝合纬线直径为0.11-0.15mm,材料采用全聚酯单丝或全尼龙单丝;所述高速宽幅生活用纸专用成形网经线密度为60-68根/cm、纬线密度为75-85根/cm。
CN201410130387.2A 2014-04-02 2014-04-02 高速宽幅生活用纸专用成形网 Pending CN103882756A (zh)