CN102796832A - Production process for leather for painting - Google Patents

Production process for leather for painting Download PDF

Info

Publication number
CN102796832A
CN102796832A CN2012103132446A CN201210313244A CN102796832A CN 102796832 A CN102796832 A CN 102796832A CN 2012103132446 A CN2012103132446 A CN 2012103132446A CN 201210313244 A CN201210313244 A CN 201210313244A CN 102796832 A CN102796832 A CN 102796832A
Authority
CN
China
Prior art keywords
tanning
agent
leather
hide
liquid
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN2012103132446A
Other languages
Chinese (zh)
Inventor
强涛涛
李飞虎
王学川
任龙芳
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shaanxi University of Science and Technology
Original Assignee
Shaanxi University of Science and Technology
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shaanxi University of Science and Technology filed Critical Shaanxi University of Science and Technology
Priority to CN2012103132446A priority Critical patent/CN102796832A/en
Publication of CN102796832A publication Critical patent/CN102796832A/en
Pending legal-status Critical Current

Abstract

The invention relates to a production process for leather for painting. The modern leather picture does not adopt the advanced production process for leather products, has a poor manufacturing method, a complex manufacturing process and single style, has no storage stability, and has high possibility of fading. The leather for painting is prepared by the steps of soaking in water, removing meat, degreasing, liming and removing hair, removing lime, softening, soaking in acid, tanning, extracting alkali after tanning, drying, painting, coating, shaping, mounting and obtaining the finished product, so that the leather has storage stability and is not damaged by worms when being placed for a long time. Painting adopts different painting methods of Chinese painting and oil painting, so that different styles are shown. The leather subjected to painting is treated, so the leather is anti-oxidant and is not faded along with the time. Chromium is not used in the tanning process, so environmental pollution is little.

Description

A kind of drawing with the production technique of leather
Technical field
The present invention relates to a kind of Process for producing leather, be specifically related to a kind of the drawing with the production technique of leather.
Background technology
Skin is drawn a kind of artwork that artistic value is arranged very much that (having another name called the skin carve and paint) is the people of Mongols invention.Skin is being decorated with very long history, and the origin that skin is drawn can be traced back to pastoral stage, and is the most common with sheepskin map, simple decoration painting.Modern Mongolian skin is drawn except that keeping simple and unsophisticated charm, dissolves in modern nationality's skill and technique more, need form such as colored paint, painted, pure making by hand of tens procedures such as layer dyes, polishing, typing, embossment convex-concave.The skin picture makes full use of and has showed that natural leather has characteristics such as the lines flow smoothly, the structure tracing is unique, stereoscopic sensation is strong, color is soft, gives brand-new artistic treat.
It is to have making a present and upholstery of reserve value and enjoying value that skin is drawn.The artistic level that skin is drawn is very high, and it makes full use of and has showed the cortex color of the leather that natural leather had, and has characteristics such as the lines flow smoothly, and the structure tracing is unique, and stereoscopic sensation is strong, and color is soft, gives brand-new artistic treat.Even but modern skin draws and still to adopt advanced leather goods production technique, manufacture technique falls behind, complex manufacturing technology, single, the not anti-storage of style and fade easily.
Along with development of science and technology, and though modern leather on working method or the resultant leather quality all than very big leap was arranged in the past.But the skin painting making technology still rests on the method in the past, produces skin with the mode of producing handicraft and draws, and soon leather is cut into small pieces and is attached on the drawing board; Adopt manual process then; Spray paint, operation such as polishing, making method is very complicated, production efficiency is low; The attractive in appearance and integrity of drawing is not more suitable for this name of skin carve and paint in fact.
At first be not have to be fit to the Process for producing leather of directly on leather, painting in the reason of directly drawing a picture on the hide, such leather is not only wanted the whiteness height, and the thickness difference at each position and pliability are low, and the degree of packing is very high; Next is direct drawing back pigment fugitive color on leather, store after for some time pigment oxidized easily and variable color takes place, phenomenon such as fade, reduce skin image quality amount greatly.
Summary of the invention
The purpose of this invention is to provide simple, anti-storage of a kind of technology and drawing not easy to fade production technique with leather.
The technical scheme that the present invention adopted is:
A kind of drawing with the production technique of leather is characterized in that:
Realize by following steps:
Step 1: immersion:
Place its quality 2-6 30-35 ℃ of immersion liquid discontinuous doubly to rotate 12-24h hide;
Step 2: fleshing:
Hide after the immersion of immersion liquid is carried out mechanical fleshing to be handled;
Step 3: degreasing:
Hide behind the fleshing is placed its quality 2-6 35-40 ℃ of degreasing fluid doubly, intermittently rotate 1-4h;
Step 4: liming depilation:
Hide after the degreasing is placed its quality 1-3 35-40 ℃ of liming liquid doubly, intermittently rotate 12-24h;
Step 5: deliming:
Hide after the liming is placed its quality 0.5-2 25-35 ℃ of deliming liquid doubly, intermittently rotate 1-4h;
Step 6: softening:
Hide behind the deliming is placed its quality 1-3 25-35 ℃ of bating liquor doubly, intermittently rotate 1-4h;
Step 7: pickling:
Hide behind the deliming is placed its quality 1-3 25-35 ℃ of pickling liquid doubly, intermittently rotate 1-4h;
Step 8: tanning:
In pickling liquid, add tanning agent and carry out tanning, tanning time 2-6h;
Step 9: carry alkali after the tanning:
The sodium bicarbonate that in tanned liquid, adds tare weight 1%-10% is carried alkali, carries alkali time 1-5h, leaves standstill 12-24h after carrying alkali;
Step 10: drying:
The stretching shady and cool place of the method Air drying that leather behind the alkali uses toggling is carried in tanning, time of drying 12-36h;
Step 11: drawing:
Hide behind the finish-drying is carried out deburring, make hide edge uniformity, directly on hide, paint then;
Step 12: cover with paint, lacquer, colour wash, etc.:
Carry out polished finish after fully drying Deng pigment, make the color and luster of drawing more bright;
Step 11: typing:
With the crust leather excess pressure roller after covering with paint, lacquer, colour wash, etc., it is more firm that its coating and decorating material is combined;
Step 12: mounting:
Crust leather mounting after the ironing in photo frame, is obtained finished product.
In the step 1, comprise the chlorinated lime that accounts for tare weight 0.1%-0.5%, the soda ash of 1%-5%, the grease-removing agent of 0.1%-1.0%, the soaking enzyme of 0.1%-0.5%, the immersion auxiliary agent of 1%-5% in the described immersion liquid.
In the step 3, comprise the soda ash that accounts for tare weight 0.5%-1.5%, the prozyme of 0.1%-1.0%, the permeate agent of 0.5%-1.5% and the grease-removing agent of 2%-6% in the described degreasing fluid.
In the step 4, contain the lime of tare weight 1.0%-5.0%, the Sodium sulfhydrate of 0.1%-1.0%, the sodium sulphite of 0.1%-1.0%, the auxiliary liming agent of 0.5%-1.5% and the grease-removing agent of 1%-4% in the described liming liquid.
In the step 5, contain the deliming agent of tare weight 0.1%-1.0%, the grease-removing agent of 0.1%-1.0%, the ammonium sulfate of 0.5%-1.5% in the described deliming liquid.
In the step 6, contain the ammonium sulfate of tare weight 0.1%-1.0%, the macerating enzyme of 0.1%-1.0%, the grease-removing agent of 0.5%-1.5% in the described bating liquor.
In the step 7, contain the salt of tare weight 5%-15%, the fatting agent of 0.1%-1.0%, the formic acid of 0.1%-1.5% in the described pickling liquid.
In the step 8, described tanning agent is oxazolidine tanning agent, LUTARALDEHYDE tanning agent, organophosphorus tanning agent, aluminum tanning agent or the zirconium tanning agent of tare weight 1%-5%;
When using the tanning of oxazolidine tanning agent, add oxazolidine after the pickling before pH between 3.0-3.5, carry alkali after pH between 7.5-8.0; When using the tanning of LUTARALDEHYDE tanning agent, add after the pickling that pH is 3.0 before the LUTARALDEHYDE, carry alkali after pH between 7.5-8.5; When using the tanning of organophosphorus tanning agent, add after the pickling that pH is 3.5 before the organophosphorus, carry that pH is 6.0 behind the alkali; When using aluminum tanning system, adding the preceding pH of aluminum tanning agent after the pickling is 3.0, carries that pH is 3.8 behind the alkali; When using zirconium tanning system, adding the preceding pH of zirconium tanning agent after the pickling is 2.5, carries that pH is 3.8 behind the alkali.
The present invention has the following advantages:
Can produce the leather of anti-storage, can not produce phenomenon such as damage by worms because of time of its placement is long; Thereby adopt Chinese painting, the different drawing means of oil painting to paint and represent different-style; Leather behind the drawing is carried out specific aim handle, antioxidant can not produce phenomenon such as fade along with the prolongation of time; Do not use chromium in the tannery, environmental pollution is little.The present invention is to the shortcoming employing specific aim processing of skin picture in the past; The making method that novel skin is drawn is proposed; Not only can improve the defective that its complex manufacturing technology, style are single, fade easily; And through increasing its quality of means lifting such as luminance brightness, raising texture, the popularization that skin is drawn has the far-reaching influence meaning.
Embodiment
Below in conjunction with embodiment the present invention is carried out detailed explanation.
Drawing includes following step with the production technique of leather among the present invention: carry alkali → drying → drawing → covering with paint → typing → mounting → finished product after immersion → fleshing → degreasing → liming depilation → deliming → softening → pickling → tanning → tanning.Concrete steps are following:
1, a kind of drawing with the production technique of leather is characterized in that:
Realize by following steps:
Step 1: immersion:
Place its quality 2-6 30-35 ℃ of immersion liquid discontinuous doubly to rotate 12-24h hide;
Step 2: fleshing:
Hide after the immersion of immersion liquid is carried out mechanical fleshing to be handled;
Step 3: degreasing:
Hide behind the fleshing is placed its quality 2-6 35-40 ℃ of degreasing fluid doubly, intermittently rotate 1-4h;
Step 4: liming depilation:
Hide after the degreasing is placed its quality 1-3 35-40 ℃ of liming liquid doubly, intermittently rotate 12-24h;
Step 5: deliming:
Hide after the liming is placed its quality 0.5-2 25-35 ℃ of deliming liquid doubly, intermittently rotate 1-4h;
Step 6: softening:
Hide behind the deliming is placed its quality 1-3 25-35 ℃ of bating liquor doubly, intermittently rotate 1-4h;
Step 7: pickling:
Hide behind the deliming is placed its quality 1-3 25-35 ℃ of pickling liquid doubly, intermittently rotate 1-4h;
Step 8: tanning:
In pickling liquid, add tanning agent and carry out tanning, tanning time 2-6h;
Step 9: carry alkali after the tanning:
The sodium bicarbonate that in tanned liquid, adds tare weight 1%-10% is carried alkali, carries alkali time 1-5h, leaves standstill 12-24h after carrying alkali;
Step 10: drying:
The stretching shady and cool place of the method Air drying that leather behind the alkali uses toggling is carried in tanning, time of drying 12-36h;
Step 11: drawing:
Hide behind the finish-drying is carried out deburring, make hide edge uniformity, directly on hide, paint then;
Step 12: cover with paint, lacquer, colour wash, etc.:
Carry out polished finish after fully drying Deng pigment, make the color and luster of drawing more bright;
Step 11: typing:
With the crust leather excess pressure roller after covering with paint, lacquer, colour wash, etc., it is more firm that its coating and decorating material is combined;
Step 12: mounting:
Crust leather mounting after the ironing in photo frame, is obtained finished product.
In the step 1, comprise the chlorinated lime that accounts for tare weight 0.1%-0.5%, the soda ash of 1%-5%, the grease-removing agent of 0.1%-1.0%, the soaking enzyme of 0.1%-0.5%, the immersion auxiliary agent of 1%-5% in the described immersion liquid.
In the step 3, comprise the soda ash that accounts for tare weight 0.5%-1.5%, the prozyme of 0.1%-1.0%, the permeate agent of 0.5%-1.5% and the grease-removing agent of 2%-6% in the described degreasing fluid.
In the step 4, contain the lime of tare weight 1.0%-5.0%, the Sodium sulfhydrate of 0.1%-1.0%, the sodium sulphite of 0.1%-1.0%, the auxiliary liming agent of 0.5%-1.5% and the grease-removing agent of 1%-4% in the described liming liquid.
In the step 5, contain the deliming agent of tare weight 0.1%-1.0%, the grease-removing agent of 0.1%-1.0%, the ammonium sulfate of 0.5%-1.5% in the described deliming liquid.
In the step 6, contain the ammonium sulfate of tare weight 0.1%-1.0%, the macerating enzyme of 0.1%-1.0%, the grease-removing agent of 0.5%-1.5% in the described bating liquor.
In the step 7, contain the salt of tare weight 5%-15%, the fatting agent of 0.1%-1.0%, the formic acid of 0.1%-1.5% in the described pickling liquid.
In the step 8, described tanning agent is oxazolidine tanning agent, LUTARALDEHYDE tanning agent, organophosphorus tanning agent, aluminum tanning agent or the zirconium tanning agent of tare weight 1%-5%;
When using the tanning of oxazolidine tanning agent, add oxazolidine after the pickling before pH between 3.0-3.5, carry alkali after pH between 7.5-8.0; When using the tanning of LUTARALDEHYDE tanning agent, add after the pickling that pH is 3.0 before the LUTARALDEHYDE, carry alkali after pH between 7.5-8.5; When using the tanning of organophosphorus tanning agent, add after the pickling that pH is 3.5 before the organophosphorus, carry that pH is 6.0 behind the alkali; When using aluminum tanning system, adding the preceding pH of aluminum tanning agent after the pickling is 3.0, carries that pH is 3.8 behind the alkali; When using zirconium tanning system, adding the preceding pH of zirconium tanning agent after the pickling is 2.5, carries that pH is 3.8 behind the alkali.
Through the practical implementation instance the present invention is described in detail explanation below.
Embodiment 1:
Step 1: immersion:
Place 30 ℃ of immersion liquid discontinuous of 2 times of its quality to rotate 12h hide;
Step 2: fleshing:
Hide after the immersion of immersion liquid is carried out mechanical fleshing to be handled;
Step 3: degreasing:
Hide behind the fleshing is placed 35 ℃ of degreasing fluids of 2 times of its quality, intermittently rotate 1h;
Step 4: liming depilation:
Hide after the degreasing is placed 35 ℃ of liming liquid of 1 times of its quality, intermittently rotate 12h;
Step 5: deliming:
Hide after the liming is placed 25 ℃ of deliming liquids of 0.5 times of its quality, measure pH after intermittently rotating 1h;
Step 6: softening:
Hide behind the deliming is placed 25 ℃ of bating liquors of 1 times of its quality, intermittently rotate 1h;
Step 7: pickling:
Hide behind the deliming is placed 25 ℃ of pickling liquid of 1 times of its quality, measure pH after intermittently rotating 1h;
Step 8: tanning:
In pickling liquid, add tanning agent and carry out tanning, tanning time 2h;
Step 9: carry alkali after the tanning:
The sodium bicarbonate that in tanned liquid, adds tare weight 1% is carried alkali, carries alkali time 1h, measures pH, leaves standstill 12h after carrying alkali;
Step 10: drying:
The stretching shady and cool place of the method Air drying that leather behind the alkali uses toggling is carried in tanning, time of drying 12h;
Step 11: drawing:
Hide behind the finish-drying is carried out deburring, make hide edge uniformity, directly on hide, paint then;
Step 12: cover with paint, lacquer, colour wash, etc.:
Carry out polished finish after fully drying Deng pigment, make the color and luster of drawing more bright;
Step 11: typing:
With the crust leather excess pressure roller after covering with paint, lacquer, colour wash, etc., it is more firm that its coating and decorating material is combined;
Step 12: mounting:
Crust leather mounting after the ironing in photo frame, is obtained finished product.
In the step 1; Comprise the chlorinated lime that accounts for tare weight 0.1%, 1% soda ash, 0.1% grease-removing agent (PA in the described immersion liquid; Sheng remittance chemical industry), 0.1% soaking enzyme (PROLIMEAN, Tag leather chemical industry), 1% immersion auxiliary agent (ACTOL NFL, ATC chemical industry).
In the step 3, comprise the grease-removing agent (DESOAGEN DN, DESAY you chemical industry) of the soda ash that accounts for tare weight 0.5%, 0.1% prozyme (DT-A448, dolantin chemical industry), 0.5% permeate agent (JFC, precious auspicious chemical industry) and 2% in the described degreasing fluid.
In the step 4, contain lime, 0.1% Sodium sulfhydrate, 0.1% sodium sulphite, 0.5% the auxiliary liming agent (ACTILIME E, ATC chemical industry) of tare weight 1.0% and 1% grease-removing agent (PX, contain converge chemical industry) in the described liming liquid.
In the step 5, contain the deliming agent (Feliderm DFA Powder, Clariant chemical industry) of tare weight 0.1%, 0.1% grease-removing agent (DESOAGEN DF, DESAY you chemical industry), 0.5% ammonium sulfate in the described deliming liquid.
In the step 6, contain the ammonium sulfate of tare weight 0.1%, 0.1% macerating enzyme (DESOBATE B2, DESAY you chemical industry), 0.5% grease-removing agent (Tergolix CA Liquid, Clariant chemical industry) in the described bating liquor.
In the step 7, contain the salt of tare weight 5%, 0.1% fatting agent (the red GLH of Ace card, Baume chemical industry), 0.1% formic acid in the described pickling liquid.
In the step 8, described tanning agent is tare weight 1%-5% De oxazolidine tanning agent ZE (DOW Chemical).When using the tanning of oxazolidine tanning agent, add oxazolidine after the pickling before pH between 3.0-3.5, carry alkali after pH between 7.5-8.0.
Embodiment 2:
Step 1: immersion:
Place 32 ℃ of immersion liquid discontinuous of 3 times of its quality to rotate 15h hide;
Step 2: fleshing:
Hide after the immersion of immersion liquid is carried out mechanical fleshing to be handled;
Step 3: degreasing:
Hide behind the fleshing is placed 37 ℃ of degreasing fluids of 3 times of its quality, intermittently rotate 1h;
Step 4: liming depilation:
Hide after the degreasing is placed 36 ℃ of liming liquid of 1 times of its quality, intermittently rotate 15h;
Step 5: deliming:
Hide after the liming is placed 28 ℃ of deliming liquids of 0.9 times of its quality, measure pH after intermittently rotating 1h;
Step 6: softening:
Hide behind the deliming is placed 28 ℃ of bating liquors of 1 times of its quality, intermittently rotate 1h;
Step 7: pickling:
Hide behind the deliming is placed 28 ℃ of pickling liquid of 1 times of its quality, measure pH after intermittently rotating 1h;
Step 8: tanning:
In pickling liquid, add tanning agent and carry out tanning, tanning time 3h;
Step 9: carry alkali after the tanning:
The sodium bicarbonate that in tanned liquid, adds tare weight 4% is carried alkali, carries alkali time 2h, measures pH, leaves standstill 15h after carrying alkali;
Step 10: drying:
The stretching shady and cool place of the method Air drying that leather behind the alkali uses toggling is carried in tanning, time of drying 18h;
Step 11: drawing:
Hide behind the finish-drying is carried out deburring, make hide edge uniformity, directly on hide, paint then;
Step 12: cover with paint, lacquer, colour wash, etc.:
Carry out polished finish after fully drying Deng pigment, make the color and luster of drawing more bright;
Step 11: typing:
With the crust leather excess pressure roller after covering with paint, lacquer, colour wash, etc., it is more firm that its coating and decorating material is combined;
Step 12: mounting:
Crust leather mounting after the ironing in photo frame, is obtained finished product.
In the step 1; Comprise the chlorinated lime that accounts for tare weight 0.2%, 2% soda ash, 0.4% grease-removing agent (PA in the described immersion liquid; Sheng remittance chemical industry), 0.2% soaking enzyme (PROLIMEAN, Tag leather chemical industry), 2% immersion auxiliary agent (ACTOL NFL, ATC chemical industry).
In the step 3, comprise the grease-removing agent (DESOAGEN DN, DESAY you chemical industry) of the soda ash that accounts for tare weight 0.8%, 0.4% prozyme (DT-A448, dolantin chemical industry), 0.8% permeate agent (JFC, precious auspicious chemical industry) and 3% in the described degreasing fluid.
In the step 4, contain lime, 0.4% Sodium sulfhydrate, 0.4% sodium sulphite, 0.8% the auxiliary liming agent (ACTILIME E, ATC chemical industry) of tare weight 2.0% and 1% grease-removing agent (PX, contain converge chemical industry) in the described liming liquid.
In the step 5, contain the deliming agent (Feliderm DFA Powder, Clariant chemical industry) of tare weight 0.4%, 0.4% grease-removing agent (DESOAGEN DF, DESAY you chemical industry), 0.8% ammonium sulfate in the described deliming liquid.
In the step 6, contain the ammonium sulfate of tare weight 0.4%, 0.4% macerating enzyme (DESOBATE B2, DESAY you chemical industry), 0.8% grease-removing agent (Tergolix CA Liquid, Clariant chemical industry) in the described bating liquor.
In the step 7, contain the salt of tare weight 8%, 0.4% fatting agent (the red GLH of Ace card, Baume chemical industry), 0.5% formic acid in the described pickling liquid.
In the step 8, described tanning agent is the LUTARALDEHYDE tanning agent PERMASOL WT (Tag chemical industry) of tare weight 2%.When using the tanning of LUTARALDEHYDE tanning agent, add LUTARALDEHYDE after the pickling before pH about 3.0, carry alkali after pH between 7.5-8.5.
Embodiment 3:
Step 1: immersion:
Place 33 ℃ of immersion liquid discontinuous of 4 times of its quality to rotate 18h hide;
Step 2: fleshing:
Hide after the immersion of immersion liquid is carried out mechanical fleshing to be handled;
Step 3: degreasing:
Hide behind the fleshing is placed 38 ℃ of degreasing fluids of 4 times of its quality, intermittently rotate 2h;
Step 4: liming depilation:
Hide after the degreasing is placed 37 ℃ of liming liquid of 2 times of its quality, intermittently rotate 18h;
Step 5: deliming:
Hide after the liming is placed 31 ℃ of deliming liquids of 1.3 times of its quality, measure pH after intermittently rotating 2h;
Step 6: softening:
Hide behind the deliming is placed 31 ℃ of bating liquors of 2 times of its quality, intermittently rotate 2h;
Step 7: pickling:
Hide behind the deliming is placed 31 ℃ of pickling liquid of 2 times of its quality, measure pH after intermittently rotating 2h;
Step 8: tanning:
In pickling liquid, add tanning agent and carry out tanning, tanning time 4h;
Step 9: carry alkali after the tanning:
The sodium bicarbonate that in tanned liquid, adds tare weight 6% is carried alkali, carries alkali time 3h, measures pH, leaves standstill 18h after carrying alkali;
Step 10: drying:
The stretching shady and cool place of the method Air drying that leather behind the alkali uses toggling is carried in tanning, time of drying 24h;
Step 11: drawing:
Hide behind the finish-drying is carried out deburring, make hide edge uniformity, directly on hide, paint then;
Step 12: cover with paint, lacquer, colour wash, etc.:
Carry out polished finish after fully drying Deng pigment, make the color and luster of drawing more bright;
Step 11: typing:
With the crust leather excess pressure roller after covering with paint, lacquer, colour wash, etc., it is more firm that its coating and decorating material is combined;
Step 12: mounting:
Crust leather mounting after the ironing in photo frame, is obtained finished product.
In the step 1; Comprise the chlorinated lime that accounts for tare weight 0.3%, 3% soda ash, 0.6% grease-removing agent (PA in the described immersion liquid; Sheng remittance chemical industry), 0.3% soaking enzyme (PROLIMEAN, Tag leather chemical industry), 3% immersion auxiliary agent (ACTOL NFL, ATC chemical industry).
In the step 3, comprise the grease-removing agent (DESOAGEN DN, DESAY you chemical industry) of the soda ash that accounts for tare weight 1.1%, 0.6% prozyme (DT-A448, dolantin chemical industry), 1.1% permeate agent (JFC, precious auspicious chemical industry) and 4% in the described degreasing fluid.
In the step 4, contain lime, 0.6% Sodium sulfhydrate, 0.6% sodium sulphite, 1.1% the auxiliary liming agent (ACTILIME E, ATC chemical industry) of tare weight 3.0% and 2% grease-removing agent (PX, contain converge chemical industry) in the described liming liquid.
In the step 5, contain the deliming agent (Feliderm DFA Powder, Clariant chemical industry) of tare weight 0.6%, 0.6% grease-removing agent (DESOAGEN DF, DESAY you chemical industry), 1.1% ammonium sulfate in the described deliming liquid.
In the step 6, contain the ammonium sulfate of tare weight 0.6%, 0.6% macerating enzyme (DESOBATE B2, DESAY you chemical industry), 1.1% grease-removing agent (Tergolix CA Liquid, Clariant chemical industry) in the described bating liquor.
In the step 7, contain the salt of tare weight 11%, 0.6% fatting agent (the red GLH of Ace card, Baume chemical industry), 0.9% formic acid in the described pickling liquid.
In the step 8, described tanning agent is the organophosphorus tanning agent DESOTAN NOC (DESAY's that chemical industry) of tare weight 3%.When using the tanning of organophosphorus tanning agent, add organophosphorus after the pickling before pH about 3.5, carry alkali after pH about 6.0.
Embodiment 4:
Step 1: immersion:
Place 34 ℃ of immersion liquid discontinuous of 5 times of its quality to rotate 21h hide;
Step 2: fleshing:
Hide after the immersion of immersion liquid is carried out mechanical fleshing to be handled;
Step 3: degreasing:
Hide behind the fleshing is placed 39 ℃ of degreasing fluids of 5 times of its quality, intermittently rotate 3h;
Step 4: liming depilation:
Hide after the degreasing is placed 38 ℃ of liming liquid of 2 times of its quality, intermittently rotate 21h;
Step 5: deliming:
Hide after the liming is placed 33 ℃ of deliming liquids of 1.7 times of its quality, measure pH after intermittently rotating 3h;
Step 6: softening:
Hide behind the deliming is placed 33 ℃ of bating liquors of 2 times of its quality, intermittently rotate 3h;
Step 7: pickling:
Hide behind the deliming is placed 33 ℃ of pickling liquid of 2 times of its quality, measure pH after intermittently rotating 3h;
Step 8: tanning:
In pickling liquid, add tanning agent and carry out tanning, tanning time 5h;
Step 9: carry alkali after the tanning:
The sodium bicarbonate that in tanned liquid, adds tare weight 8% is carried alkali, carries alkali time 4h, measures pH, leaves standstill 21h after carrying alkali;
Step 10: drying:
The stretching shady and cool place of the method Air drying that leather behind the alkali uses toggling is carried in tanning, time of drying 30h;
Step 11: drawing:
Hide behind the finish-drying is carried out deburring, make hide edge uniformity, directly on hide, paint then;
Step 12: cover with paint, lacquer, colour wash, etc.:
Carry out polished finish after fully drying Deng pigment, make the color and luster of drawing more bright;
Step 11: typing:
With the crust leather excess pressure roller after covering with paint, lacquer, colour wash, etc., it is more firm that its coating and decorating material is combined;
Step 12: mounting:
Crust leather mounting after the ironing in photo frame, is obtained finished product.
In the step 1; Comprise the chlorinated lime that accounts for tare weight 0.4%, 4% soda ash, 0.8% grease-removing agent (PA in the described immersion liquid; Sheng remittance chemical industry), 0.4% soaking enzyme (PROLIMEAN, Tag leather chemical industry), 4% immersion auxiliary agent (ACTOL NFL, ATC chemical industry).
In the step 3, comprise the grease-removing agent (DESOAGEN DN, DESAY you chemical industry) of the soda ash that accounts for tare weight 1.3%, 0.8% prozyme (DT-A448, dolantin chemical industry), 1.3% permeate agent (JFC, precious auspicious chemical industry) and 5% in the described degreasing fluid.
In the step 4, contain lime, 0.8% Sodium sulfhydrate, 0.8% sodium sulphite, 1.3% the auxiliary liming agent (ACTILIME E, ATC chemical industry) of tare weight 4.0% and 3% grease-removing agent (PX, contain converge chemical industry) in the described liming liquid.
In the step 5, contain the deliming agent (Feliderm DFA Powder, Clariant chemical industry) of tare weight 0.8%, 0.8% grease-removing agent (DESOAGEN DF, DESAY you chemical industry), 1.3% ammonium sulfate in the described deliming liquid.
In the step 6, contain the ammonium sulfate of tare weight 0.8%, 0.8% macerating enzyme (DESOBATE B2, DESAY you chemical industry), 1.3% grease-removing agent (Tergolix CA Liquid, Clariant chemical industry) in the described bating liquor.
In the step 7, contain the salt of tare weight 13%, 0.8% fatting agent (the red GLH of Ace card, Baume chemical industry), 1.2% formic acid in the described pickling liquid.
In the step 8, described tanning agent is the aluminum tanning agent DT-T712 (dolantin chemical industry) of tare weight 4%.When using aluminum tanning system, add the preceding pH of aluminum tanning agent after the pickling about 3.0, carry alkali after pH about 3.8.
Embodiment 5:
Step 1: immersion:
Place 35 ℃ of immersion liquid discontinuous of 6 times of its quality to rotate 24h hide;
Step 2: fleshing:
Hide after the immersion of immersion liquid is carried out mechanical fleshing to be handled;
Step 3: degreasing:
Hide behind the fleshing is placed 40 ℃ of degreasing fluids of 6 times of its quality, intermittently rotate 4h;
Step 4: liming depilation:
Hide after the degreasing is placed 40 ℃ of liming liquid of 3 times of its quality, intermittently rotate 24h;
Step 5: deliming:
Hide after the liming is placed 35 ℃ of deliming liquids of 2 times of its quality, measure pH after intermittently rotating 4h;
Step 6: softening:
Hide behind the deliming is placed 35 ℃ of bating liquors of 3 times of its quality, intermittently rotate 4h;
Step 7: pickling:
Hide behind the deliming is placed 35 ℃ of pickling liquid of 3 times of its quality, measure pH after intermittently rotating 4h;
Step 8: tanning:
In pickling liquid, add tanning agent and carry out tanning, tanning time 6h;
Step 9: carry alkali after the tanning:
The sodium bicarbonate that in tanned liquid, adds tare weight 10% is carried alkali, carries alkali time 5h, measures pH, leaves standstill 24h after carrying alkali;
Step 10: drying:
The stretching shady and cool place of the method Air drying that leather behind the alkali uses toggling is carried in tanning, time of drying 36h;
Step 11: drawing:
Hide behind the finish-drying is carried out deburring, make hide edge uniformity, directly on hide, paint then;
Step 12: cover with paint, lacquer, colour wash, etc.:
Carry out polished finish after fully drying Deng pigment, make the color and luster of drawing more bright;
Step 11: typing:
With the crust leather excess pressure roller after covering with paint, lacquer, colour wash, etc., it is more firm that its coating and decorating material is combined;
Step 12: mounting:
Crust leather mounting after the ironing in photo frame, is obtained finished product.
In the step 1; Comprise the chlorinated lime that accounts for tare weight 0.5%, 5% soda ash, 1.0% grease-removing agent (PA in the described immersion liquid; Sheng remittance chemical industry), 0.5% soaking enzyme (PROLIMEAN, Tag leather chemical industry), 5% immersion auxiliary agent (ACTOL NFL, ATC chemical industry).
In the step 3, comprise the grease-removing agent (DESOAGEN DN, DESAY you chemical industry) of the soda ash that accounts for tare weight 1.5%, 1.0% prozyme (DT-A448, dolantin chemical industry), 1.5% permeate agent (JFC, precious auspicious chemical industry) and 6% in the described degreasing fluid.
In the step 4, contain lime, 1.0% Sodium sulfhydrate, 1.0% sodium sulphite, 1.5% the auxiliary liming agent (ACTILIME E, ATC chemical industry) of tare weight 5.0% and 4% grease-removing agent (PX, contain converge chemical industry) in the described liming liquid.
In the step 5, contain the deliming agent (Feliderm DFA Powder, Clariant chemical industry) of tare weight 1.0%, 1.0% grease-removing agent (DESOAGEN DF, DESAY you chemical industry), 1.5% ammonium sulfate in the described deliming liquid.
In the step 6, contain the ammonium sulfate of tare weight 1.0%, 1.0% macerating enzyme (DESOBATE B2, DESAY you chemical industry), 1.5% grease-removing agent (Tergolix CA Liquid, Clariant chemical industry) in the described bating liquor.
In the step 7, contain the salt of tare weight 15%, 1.0% fatting agent (the red GLH of Ace card, Baume chemical industry), 1.5% formic acid in the described pickling liquid.
In the step 8, described tanning agent is the zirconium tanning agent Tanfix SZS Powder (Clariant chemical industry) of tare weight 5%.When using zirconium tanning system, add the preceding pH of zirconium tanning agent after the pickling about 2.5, carry alkali after pH about 3.8.
It is cited that content of the present invention is not limited to embodiment, and the conversion of any equivalence that those of ordinary skills take technical scheme of the present invention through reading specification sheets of the present invention is claim of the present invention and contains.
The leather whiteness that present method is produced is about 60 degree, and the thickness difference at each position is in 5%, and elongation is about 50% in the 8MPa left and right sides for tensile strength, and tear strength is about 35N/mm.The general chromic tanning that adopts is produced leather, and the crust leather of chrome tanning is a turquoise, be unfavorable for the painting contrast of color and the infiltration of drawing pigment, and the crust leather that present method is produced is a white, has the drawing paper of whiteness; Secondly the tanned leather of ordinary method is softer, the different sites uneven thickness, the quality behind the influence drawing, the crust leather that present method is produced has the hard characteristics of leather body, each position consistency of thickness of tiling back, tear and tensile strength little, be similar to the drawing paper; At last, present method is after tanning, to paint, and covers with paint, lacquer, colour wash, etc. afterwards, has effectively protected drawing pigment, is difficult for taking place the variable color and the phenomenon of fading.

Claims (8)

1. paint with the production technique of leather for one kind, it is characterized in that:
Realize by following steps:
Step 1: immersion:
Place its quality 2-6 30-35 ℃ of immersion liquid discontinuous doubly to rotate 12-24h hide;
Step 2: fleshing:
Hide after the immersion of immersion liquid is carried out mechanical fleshing to be handled;
Step 3: degreasing:
Hide behind the fleshing is placed its quality 2-6 35-40 ℃ of degreasing fluid doubly, intermittently rotate 1-4h;
Step 4: liming depilation:
Hide after the degreasing is placed its quality 1-3 35-40 ℃ of liming liquid doubly, intermittently rotate 12-24h;
Step 5: deliming:
Hide after the liming is placed its quality 0.5-2 25-35 ℃ of deliming liquid doubly, intermittently rotate 1-4h;
Step 6: softening:
Hide behind the deliming is placed its quality 1-3 25-35 ℃ of bating liquor doubly, intermittently rotate 1-4h;
Step 7: pickling:
Hide behind the deliming is placed its quality 1-3 25-35 ℃ of pickling liquid doubly, intermittently rotate 1-4h;
Step 8: tanning:
In pickling liquid, add tanning agent and carry out tanning, tanning time 2-6h;
Step 9: carry alkali after the tanning:
The sodium bicarbonate that in tanned liquid, adds tare weight 1%-10% is carried alkali, carries alkali time 1-5h, leaves standstill 12-24h after carrying alkali;
Step 10: drying:
The stretching shady and cool place of the method Air drying that leather behind the alkali uses toggling is carried in tanning, time of drying 12-36h;
Step 11: drawing:
Hide behind the finish-drying is carried out deburring, make hide edge uniformity, directly on hide, paint then;
Step 12: cover with paint, lacquer, colour wash, etc.:
Carry out polished finish after fully drying Deng pigment, make the color and luster of drawing more bright;
Step 11: typing:
With the crust leather excess pressure roller after covering with paint, lacquer, colour wash, etc., it is more firm that its coating and decorating material is combined;
Step 12: mounting:
Crust leather mounting after the ironing in photo frame, is obtained finished product.
2. a kind of the drawing with the production technique of leather according to claim 1 is characterized in that:
In the step 1, comprise the chlorinated lime that accounts for tare weight 0.1%-0.5%, the soda ash of 1%-5%, the grease-removing agent of 0.1%-1.0%, the soaking enzyme of 0.1%-0.5%, the immersion auxiliary agent of 1%-5% in the described immersion liquid.
3. a kind of the drawing with the production technique of leather according to claim 1 and 2 is characterized in that:
In the step 3, comprise the soda ash that accounts for tare weight 0.5%-1.5%, the prozyme of 0.1%-1.0%, the permeate agent of 0.5%-1.5% and the grease-removing agent of 2%-6% in the described degreasing fluid.
4. a kind of the drawing with the production technique of leather according to claim 3 is characterized in that:
In the step 4, contain the lime of tare weight 1.0%-5.0%, the Sodium sulfhydrate of 0.1%-1.0%, the sodium sulphite of 0.1%-1.0%, the auxiliary liming agent of 0.5%-1.5% and the grease-removing agent of 1%-4% in the described liming liquid.
5. a kind of the drawing with the production technique of leather according to claim 4 is characterized in that:
In the step 5, contain the deliming agent of tare weight 0.1%-1.0%, the grease-removing agent of 0.1%-1.0%, the ammonium sulfate of 0.5%-1.5% in the described deliming liquid.
6. a kind of the drawing with the production technique of leather according to claim 5 is characterized in that:
In the step 6, contain the ammonium sulfate of tare weight 0.1%-1.0%, the macerating enzyme of 0.1%-1.0%, the grease-removing agent of 0.5%-1.5% in the described bating liquor.
7. a kind of the drawing with the production technique of leather according to claim 6 is characterized in that:
In the step 7, contain the salt of tare weight 5%-15%, the fatting agent of 0.1%-1.0%, the formic acid of 0.1%-1.5% in the described pickling liquid.
8. a kind of the drawing with the production technique of leather according to claim 7 is characterized in that:
In the step 8, described tanning agent is oxazolidine tanning agent, LUTARALDEHYDE tanning agent, organophosphorus tanning agent, aluminum tanning agent or the zirconium tanning agent of tare weight 1%-5%;
When using the tanning of oxazolidine tanning agent, add oxazolidine after the pickling before pH between 3.0-3.5, carry alkali after pH between 7.5-8.0; When using the tanning of LUTARALDEHYDE tanning agent, add after the pickling that pH is 3.0 before the LUTARALDEHYDE, carry alkali after pH between 7.5-8.5; When using the tanning of organophosphorus tanning agent, add after the pickling that pH is 3.5 before the organophosphorus, carry that pH is 6.0 behind the alkali; When using aluminum tanning system, adding the preceding pH of aluminum tanning agent after the pickling is 3.0, carries that pH is 3.8 behind the alkali; When using zirconium tanning system, adding the preceding pH of zirconium tanning agent after the pickling is 2.5, carries that pH is 3.8 behind the alkali.
CN2012103132446A 2012-08-30 2012-08-30 Production process for leather for painting Pending CN102796832A (en)