CN107090527A - Tanning agent and its crocodile skin process for tanning for crocodile skin - Google Patents

Tanning agent and its crocodile skin process for tanning for crocodile skin Download PDF

Info

Publication number
CN107090527A
CN107090527A CN201710452093.5A CN201710452093A CN107090527A CN 107090527 A CN107090527 A CN 107090527A CN 201710452093 A CN201710452093 A CN 201710452093A CN 107090527 A CN107090527 A CN 107090527A
Authority
CN
China
Prior art keywords
parts
tanning
crocodile skin
tanning agent
crocodile
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
CN201710452093.5A
Other languages
Chinese (zh)
Inventor
王星河
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Quanzhou Xincai Trade Co Ltd
Original Assignee
Quanzhou Xincai Trade Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Quanzhou Xincai Trade Co Ltd filed Critical Quanzhou Xincai Trade Co Ltd
Priority to CN201710452093.5A priority Critical patent/CN107090527A/en
Publication of CN107090527A publication Critical patent/CN107090527A/en
Withdrawn legal-status Critical Current

Abstract

The present invention relates to a kind of tanning agent for crocodile skin and its crocodile skin process for tanning, the tanning agent is made up of fatty aldehyde, resorcinol calixarenes, Lauxite, polyvinylpyrrolidone, methylene-succinic acid, double carboxyethyl amine, sodium phthalate, 2-carboxybenzaldehyde, di-n-butylamine, maleic acid and ammonium persulfate, and the process for tanning is that crocodile skin is sequentially passed through into immersion, fleshing, softening, tanning and the processing for drying process.Targetedly crocodile skin plays good tanning effect to the tanning agent of the present invention, process can effectively be simplified by carrying out tanning to crocodile skin using the tanning agent of the present invention, crocodile skin only by immersion, fleshing, softening, tanning and need to dry the processing of process and can obtain crocodile, tanning processes possess fat-reducing function to crocodile skin, process for tanning is effectively simplified, tanning efficiency is also effectively lifted, production cost is effectively reduced, and obtained crocodile possesses soft fine and smooth, wear-resisting, the elastic superperformance such as good.

Description

Tanning agent and its crocodile skin process for tanning for crocodile skin
Technical field
The present invention relates to a kind of tanning agent and its process for tanning, particularly relate to a kind of tanning agent for being particularly suitable for use in crocodile skin and its Crocodile skin process for tanning.
Background technology
Leather is through the not perishable Animal Skin of denaturation obtained by physics, the chemical process such as depilation and tanning.Leather It is made up of natural protein fibre in three dimensions close weave, there is a kind of special grain layer on its surface, with nature Graining and gloss, comfortable feel.
Current leather tanning process is complex, and such as the Chinese invention patent of Application No. 201310725180.5 is provided A kind of process for tanning goat leather by synthetic tanning agent, uses the tanning processes of its tanning agent to select skin → immersion → degreasing → water-bath → multiple Immersion → fleshing → secondary degreasing → pickling → softening → get damp again perching for tanning → neutralization → water dumping is dried →.The tanning processes are needed The processes such as multiple immersion, degreasing are wanted, technique is complex, and the tanning of leather is inefficient, production cost is high.
The content of the invention
The present invention provides a kind of tanning agent and its crocodile skin process for tanning for crocodile skin, to overcome current part tanning The problem of tanning processes that technique is present are complicated, efficiency is low, cost is high.
The present invention is adopted the following technical scheme that:
For the tanning agent of crocodile skin, the preparation of the tanning agent is made up of following raw materials by weight ratio:6~11 parts of fat Aldehyde, 4~6 parts of resorcinol calixarenes, 9~13 parts of Lauxite, 1~3 part of polyvinylpyrrolidone, 11~15 parts Methylene-succinic acid, 7~9 parts of double carboxyethyl amine, 15~17 parts of sodium phthalate, 3~6 parts of 2-carboxybenzaldehyde, 4 ~7 parts of di-n-butylamine, 5~8 parts of maleic acid and 8~11 parts of ammonium persulfate.
Further, the preparation of the tanning agent is made up of following raw materials by weight ratio:7.5~9.5 parts of fatty aldehyde, 4.5~5.5 parts of resorcinol calixarenes, 10~12 parts of Lauxite, 1.5~2.5 parts of polyvinylpyrrolidone, 12~ 14 parts of methylene-succinic acid, 7.5~8.5 parts of double carboxyethyl amine, 16~16.5 parts of sodium phthalate, 3.5~4.5 parts 2-carboxybenzaldehyde, 4.5~5.5 parts of di-n-butylamine, 6.5~7.5 parts of maleic acid and 9~10 parts of persulfuric acid Ammonium.
More specifically, the raw material proportioning of preferably following five kinds of tanning agents:
First, the preparation of the tanning agent is made up of following raw materials by weight ratio:8.5 parts of fatty aldehyde, 5 parts of resorcinol Calixarenes, 11 parts of Lauxite, 2 parts of polyvinylpyrrolidone, 13 parts of methylene-succinic acid, 8 parts of double carboxyethyl amine, 16 parts of sodium phthalate, 4.5 parts of 2-carboxybenzaldehyde, 5.5 parts of di-n-butylamine, 6.5 parts of maleic acid and 10 The ammonium persulfate of part.
Second, the preparation of the tanning agent is made up of following raw materials by weight ratio:Between 7.5 parts of fatty aldehyde, 5.5 parts Benzenediol calixarenes, 12 parts of Lauxite, 1.5 parts of polyvinylpyrrolidone, 12 parts of methylene-succinic acid, 8.5 parts Double carboxyethyl amine, 16.5 parts of sodium phthalate, 3.5 parts of 2-carboxybenzaldehyde, 4.5 parts of di-n-butylamine, 7.5 parts suitable Butene dioic acid and 9 parts of ammonium persulfate.
Third, the preparation of the tanning agent is made up of following raw materials by weight ratio:Between 9.5 parts of fatty aldehyde, 4.5 parts Benzenediol calixarenes, 10 parts of Lauxite, 2.5 parts of polyvinylpyrrolidone, 14 parts of methylene-succinic acid, 7.5 parts Double carboxyethyl amine, 16 parts of sodium phthalate, 4.5 parts of 2-carboxybenzaldehyde, 5.5 parts of di-n-butylamine, 6.5 parts of suitable fourth Enedioic acid and 9.5 parts of ammonium persulfate.
Fourth, the preparation of the tanning agent is made up of following raw materials by weight ratio:6 parts of fatty aldehyde, 6 parts of isophthalic two Phenol calixarenes, 13 parts of Lauxite, 1 part of polyvinylpyrrolidone, 11 parts of methylene-succinic acid, 9 parts of double carboxyethyls Amine, 15 parts of sodium phthalate, 6 parts of 2-carboxybenzaldehyde, 7 parts of di-n-butylamine, 8 parts of maleic acid and 11 parts Ammonium persulfate.
Fifth, the preparation of the tanning agent is made up of following raw materials by weight ratio:11 parts of fatty aldehyde, 4 parts of isophthalic Diphenol calixarenes, 9 parts of Lauxite, 3 parts of polyvinylpyrrolidone, 15 parts of methylene-succinic acid, 7 parts of double carboxyethyls Amine, 17 parts of sodium phthalate, 3 parts of 2-carboxybenzaldehyde, 4 parts of di-n-butylamine, 5 parts of maleic acid and 8 parts Ammonium persulfate.
The process for tanning of crocodile skin, crocodile skin is only handled by the following processes carried out successively:
A. soak:Plucked crocodile skin is immersed in the salt solution that PH is 4~5, soak time is 6~8 hours;
B. fleshing:The meat of crocodile skin is rooted out by fleshing machine;
C. soften:Crocodile skin is immersed in the salt solution that PH is 4~5, soak time is 15~20 minutes, then crocodile skin passes through Drain within 4~8 hours;
D. tanning:The raw material of the above-mentioned tanning agent for crocodile skin is added in organic solvent, the weight ratio of feed liquid is 1:15 ~25, crocodile skin is immersed in tanning agent solution, soak time is 28~35 hours, crocodile skin was dripped after taking out by 3~4 hours It is dry;
E. dry:Crocodile is can obtain after natural drying.
Further, above-mentioned organic solvent is ethanol, glycerine, isooctane, isopropyl ether, methyl isopropyl ketone, methyl tetrahydrochysene One or more kinds of combinations in furans, petroleum ether, trichloroacetic acid, trifluoroacetic acid.
From the above-mentioned description of this invention, compared to the prior art, the invention has the advantages that:The tan of the present invention Targetedly crocodile skin plays good tanning effect for agent, and carrying out tanning to crocodile skin using the tanning agent of the present invention can be effective Simplify process, crocodile skin only by immersion, fleshing, softening, tanning and need to dry the processing of process and can obtain crocodile, tan Process processed possesses fat-reducing function to crocodile skin, and process for tanning is effectively simplified, and tanning efficiency is also effectively lifted, production Cost is effectively reduced, and obtained crocodile possesses soft fine and smooth, wear-resisting, the elastic superperformance such as good.
Embodiment
Embodiment one
The preparation of the tanning agent is made up of following raw materials by weight ratio:8.5 parts of fatty aldehyde, 5 parts of resorcinol cup virtue Hydrocarbon, 11 parts of Lauxite, 2 parts of polyvinylpyrrolidone, 13 parts of methylene-succinic acid, 8 parts of double carboxyethyl amine, 16 parts Sodium phthalate, 4.5 parts of 2-carboxybenzaldehyde, 5.5 parts of di-n-butylamine, 6.5 parts of maleic acid and 10 parts Ammonium persulfate.
Process for tanning using the crocodile skin of the tanning agent of present embodiment is, following works of the crocodile skin only by carrying out successively Sequence processing:
A. soak:Plucked crocodile skin is immersed in the salt solution that PH is 4.5, soak time is 6 hours;
B. fleshing:The meat of crocodile skin is rooted out by fleshing machine;
C. soften:Crocodile skin is immersed in the salt solution that PH is 4.5, soak time is 15~17 minutes, and then crocodile skin passes through 4 Drain within~8 hours;
D. tanning:The raw material of the tanning agent for crocodile skin of present embodiment is added in organic solvent, the weight ratio of feed liquid For 1:23~25, crocodile skin is immersed in tanning agent solution, soak time is 28~30 hours, and crocodile skin is small by 3 after taking out When drain;Organic solvent is ethanol and glycerine;
E. dry:Crocodile is can obtain after natural drying.
Present embodiment is optimal embodiment, and targetedly crocodile skin plays good tan to the tanning agent of present embodiment Make and use, tanning is carried out to crocodile skin using the tanning agent of the present invention can effectively simplify process, and crocodile skin need to only pass through immersion, go Meat, softening, tanning and dry the processing of process and can obtain crocodile, tanning processes possess fat-reducing function, tan to crocodile skin Technique processed is effectively simplified, and tanning efficiency is also effectively lifted, and production cost is effectively reduced, and obtained crocodile Fish skin leather possesses soft fine and smooth, wear-resisting, the elastic superperformance such as good.
Embodiment two
The preparation of the tanning agent of present embodiment is made up of following raw materials by weight ratio:7.5 parts of fatty aldehyde, 5.5 parts Resorcinol calixarenes, 12 parts of Lauxite, 1.5 parts of polyvinylpyrrolidone, 12 parts of methylene-succinic acid, 8.5 parts Double carboxyethyl amine, 16.5 parts of sodium phthalate, 3.5 parts of 2-carboxybenzaldehyde, 4.5 parts of di-n-butylamine, 7.5 parts Maleic acid and 9 parts of ammonium persulfate.
Process for tanning using the crocodile skin of the tanning agent of present embodiment is, following works of the crocodile skin only by carrying out successively Sequence processing:
A. soak:Plucked crocodile skin is immersed in the salt solution that PH is 5, soak time is 8 hours;
B. fleshing:The meat of crocodile skin is rooted out by fleshing machine;
C. soften:Crocodile skin is immersed in the salt solution that PH is 5, soak time is 20 minutes, and then crocodile skin is small by 4~8 When drain;
D. tanning:The raw material of the tanning agent for crocodile skin of present embodiment is added in organic solvent, the weight ratio of feed liquid For 1:22~24, crocodile skin is immersed in tanning agent solution, soak time is 29~32 hours, by 3~4 after crocodile skin taking-up Hour drains;Organic solvent is glycerine and isooctane;
E. dry:Crocodile is can obtain after natural drying.
Embodiment three
The preparation of the tanning agent of present embodiment is made up of following raw materials by weight ratio:9.5 parts of fatty aldehyde, 4.5 parts Resorcinol calixarenes, 10 parts of Lauxite, 2.5 parts of polyvinylpyrrolidone, 14 parts of methylene-succinic acid, 7.5 parts Double carboxyethyl amine, 16 parts of sodium phthalate, 4.5 parts of 2-carboxybenzaldehyde, 5.5 parts of di-n-butylamine, 6.5 parts suitable Butene dioic acid and 9.5 parts of ammonium persulfate.
Process for tanning using the crocodile skin of the tanning agent of present embodiment is, following works of the crocodile skin only by carrying out successively Sequence processing:
A. soak:Plucked crocodile skin is immersed in the salt solution that PH is 4, soak time is 64 hours;
B. fleshing:The meat of crocodile skin is rooted out by fleshing machine;
C. soften:Crocodile skin is immersed in the salt solution that PH is 4, soak time is 15 minutes, and then crocodile skin is small by 4~8 When drain;
D. tanning:The raw material of the tanning agent for crocodile skin of present embodiment is added in organic solvent, the weight ratio of feed liquid For 1:15~18, crocodile skin is immersed in tanning agent solution, soak time is 28~30 hours, by 3~4 after crocodile skin taking-up Hour drains;Organic solvent is glycerine;
E. dry:Crocodile is can obtain after natural drying.
Embodiment four
The preparation of the tanning agent of present embodiment is made up of following raw materials by weight ratio:6 parts of fatty aldehyde, 6 parts of isophthalic Diphenol calixarenes, 13 parts of Lauxite, 1 part of polyvinylpyrrolidone, 11 parts of methylene-succinic acid, 9 parts of double carboxylic second Base amine, 15 parts of sodium phthalate, 6 parts of 2-carboxybenzaldehyde, 7 parts of di-n-butylamine, 8 parts of maleic acid and 11 parts Ammonium persulfate.
Process for tanning using the crocodile skin of the tanning agent of present embodiment is, following works of the crocodile skin only by carrying out successively Sequence processing:
A. soak:Plucked crocodile skin is immersed in the salt solution that PH is 4.5, soak time is 7 hours;
B. fleshing:The meat of crocodile skin is rooted out by fleshing machine;
C. soften:Crocodile skin is immersed in the salt solution that PH is 4.5, soak time is 18 minutes, then crocodile skin passes through 4~8 Hour drains;
D. tanning:The raw material of the tanning agent for crocodile skin of present embodiment is added in organic solvent, the weight ratio of feed liquid For 1:18~19, crocodile skin is immersed in tanning agent solution, soak time is 30~33 hours, by 3~4 after crocodile skin taking-up Hour drains;Organic solvent is methyltetrahydrofuran and petroleum ether;
E. dry:Crocodile is can obtain after natural drying.
Embodiment five
The preparation of the tanning agent of present embodiment is made up of following raw materials by weight ratio:11 parts of fatty aldehyde, 4 parts of isophthalic Diphenol calixarenes, 9 parts of Lauxite, 3 parts of polyvinylpyrrolidone, 15 parts of methylene-succinic acid, 7 parts of double carboxyethyls Amine, 17 parts of sodium phthalate, 3 parts of 2-carboxybenzaldehyde, 4 parts of di-n-butylamine, 5 parts of maleic acid and 8 parts Ammonium persulfate.
Process for tanning using the crocodile skin of the tanning agent of present embodiment is, following works of the crocodile skin only by carrying out successively Sequence processing:
A. soak:Plucked crocodile skin is immersed in the salt solution that PH is 4.5, soak time is 8 hours;
B. fleshing:The meat of crocodile skin is rooted out by fleshing machine;
C. soften:Crocodile skin is immersed in the salt solution that PH is 4.5, soak time is 20 minutes, then crocodile skin passes through 4~8 Hour drains;
D. tanning:The raw material of the tanning agent for crocodile skin of present embodiment is added in organic solvent, the weight ratio of feed liquid For 1:21~23, crocodile skin is immersed in tanning agent solution, soak time is 33~35 hours, by 3~4 after crocodile skin taking-up Hour drains;Organic solvent is trichloroacetic acid;
E. dry:Crocodile is can obtain after natural drying.
Embodiment six
The preparation of the tanning agent of present embodiment is made up of following raw materials by weight ratio:8.5 parts of fatty aldehyde, 5.5 parts Resorcinol calixarenes, 11.5 parts of Lauxite, 2.5 parts of polyvinylpyrrolidone, 12.5 parts of methylene-succinic acid, 8 Part double carboxyethyl amine, 16 parts of sodium phthalate, 4 parts of 2-carboxybenzaldehyde, 4.5 parts of di-n-butylamine, 7.2 parts suitable Butene dioic acid and 9.8 parts of ammonium persulfate.
Process for tanning using the crocodile skin of the tanning agent of present embodiment is, following works of the crocodile skin only by carrying out successively Sequence processing:
A. soak:Plucked crocodile skin is immersed in the salt solution that PH is 4.5, soak time is 6.5 hours;
B. fleshing:The meat of crocodile skin is rooted out by fleshing machine;
C. soften:Crocodile skin is immersed in the salt solution that PH is 4.5, soak time is 17 minutes, then crocodile skin passes through 4~8 Hour drains;
D. tanning:The raw material of the tanning agent for crocodile skin of present embodiment is added in organic solvent, the weight ratio of feed liquid For 1:18~21, crocodile skin is immersed in tanning agent solution, soak time is 29~30 hours, by 3~4 after crocodile skin taking-up Hour drains;Organic solvent is glycerine, trichloroacetic acid and trifluoroacetic acid;
E. dry:Crocodile is can obtain after natural drying.
Embodiment seven
The preparation of the tanning agent of present embodiment is made up of following raw materials by weight ratio:Between 9 parts of fatty aldehyde, 5.2 parts Benzenediol calixarenes, 10.5 parts of Lauxite, 1.8 parts of polyvinylpyrrolidone, 13.3 parts of methylene-succinic acid, 7.8 Part double carboxyethyl amine, 16.3 parts of sodium phthalate, 4.2 parts of 2-carboxybenzaldehyde, 5.2 parts of di-n-butylamine, 7.2 parts Maleic acid and 9 parts of ammonium persulfate.
Process for tanning using the crocodile skin of the tanning agent of present embodiment is, following works of the crocodile skin only by carrying out successively Sequence processing:
A. soak:Plucked crocodile skin is immersed in the salt solution that PH is 4.5, soak time is 7.5 hours;
B. fleshing:The meat of crocodile skin is rooted out by fleshing machine;
C. soften:Crocodile skin is immersed in the salt solution that PH is 4.5, soak time is 15 minutes, then crocodile skin passes through 4~8 Hour drains;
D. tanning:The raw material of the tanning agent for crocodile skin of present embodiment is added in organic solvent, the weight ratio of feed liquid For 1:15~17, crocodile skin is immersed in tanning agent solution, soak time is 30~32 hours, by 3~4 after crocodile skin taking-up Hour drains;Organic solvent is isooctane, isopropyl ether and methyltetrahydrofuran;
E. dry:Crocodile is can obtain after natural drying.
The embodiment of the present invention is above are only, but the design concept of the present invention is not limited thereto, it is all to utilize this Conceive the change that unsubstantiality is carried out to the present invention, the behavior for invading the scope of the present invention all should be belonged to.

Claims (9)

1. the tanning agent for crocodile skin, it is characterised in that the preparation of the tanning agent is made up of following raw materials by weight ratio:6 ~11 parts of fatty aldehyde, 4~6 parts of resorcinol calixarenes, 9~13 parts of Lauxite, 1~3 part of polyvinylpyrrolidine Ketone, 11~15 parts of methylene-succinic acid, 7~9 parts of double carboxyethyl amine, 15~17 parts of sodium phthalate, 3~6 parts 2-carboxybenzaldehyde, 4~7 parts of di-n-butylamine, 5~8 parts of maleic acid and 8~11 parts of ammonium persulfate.
2. it is used for the tanning agent of crocodile skin as claimed in claim 1, it is characterised in that the preparation of the tanning agent is by by weight ratio Following raw materials constitute:7.5~9.5 parts of fatty aldehyde, 4.5~5.5 parts of resorcinol calixarenes, 10~12 parts of ureaformaldehyde tree Fat, 1.5~2.5 parts of polyvinylpyrrolidone, 12~14 parts of methylene-succinic acid, 7.5~8.5 parts of double carboxyethyl amine, 16~16.5 parts of sodium phthalate, 3.5~4.5 parts of 2-carboxybenzaldehyde, 4.5~5.5 parts of di-n-butylamine, 6.5~ 7.5 parts of maleic acid and 9~10 parts of ammonium persulfate.
3. it is used for the tanning agent of crocodile skin as claimed in claim 2, it is characterised in that the preparation of the tanning agent is by by weight ratio Following raw materials constitute:8.5 parts of fatty aldehyde, 5 parts of resorcinol calixarenes, 11 parts of Lauxite, 2 parts of polyethylene pyrrole Pyrrolidone, 13 parts of methylene-succinic acid, 8 parts of double carboxyethyl amine, 16 parts of sodium phthalate, 4.5 parts of adjacent carboxyl benzene Formaldehyde, 5.5 parts of di-n-butylamine, 6.5 parts of maleic acid and 10 parts of ammonium persulfate.
4. it is used for the tanning agent of crocodile skin as claimed in claim 2, it is characterised in that the preparation of the tanning agent is by by weight ratio Following raw materials constitute:7.5 parts of fatty aldehyde, 5.5 parts of resorcinol calixarenes, 12 parts of Lauxite, 1.5 parts of poly- second Alkene pyrrolidone, 12 parts of methylene-succinic acid, 8.5 parts of double carboxyethyl amine, 16.5 parts of sodium phthalate, 3.5 parts 2-carboxybenzaldehyde, 4.5 parts of di-n-butylamine, 7.5 parts of maleic acid and 9 parts of ammonium persulfate.
5. it is used for the tanning agent of crocodile skin as claimed in claim 2, it is characterised in that the preparation of the tanning agent is by by weight ratio Following raw materials constitute:9.5 parts of fatty aldehyde, 4.5 parts of resorcinol calixarenes, 10 parts of Lauxite, 2.5 parts of poly- second Alkene pyrrolidone, 14 parts of methylene-succinic acid, 7.5 parts of double carboxyethyl amine, 16 parts of sodium phthalate, 4.5 parts of neighbour Carboxyl benzaldehyde, 5.5 parts of di-n-butylamine, 6.5 parts of maleic acid and 9.5 parts of ammonium persulfate.
6. it is used for the tanning agent of crocodile skin as claimed in claim 1, it is characterised in that the preparation of the tanning agent is by by weight ratio Following raw materials constitute:6 parts of fatty aldehyde, 6 parts of resorcinol calixarenes, 13 parts of Lauxite, 1 part of polyvinyl pyrrole Alkanone, 11 parts of methylene-succinic acid, 9 parts of double carboxyethyl amine, 15 parts of sodium phthalate, 6 parts of 2-carboxybenzaldehyde, 7 parts of di-n-butylamine, 8 parts of maleic acid and 11 parts of ammonium persulfate.
7. it is used for the tanning agent of crocodile skin as claimed in claim 1, it is characterised in that the preparation of the tanning agent is by by weight ratio Following raw materials constitute:11 parts of fatty aldehyde, 4 parts of resorcinol calixarenes, 9 parts of Lauxite, 3 parts of polyvinyl pyrrole Alkanone, 15 parts of methylene-succinic acid, 7 parts of double carboxyethyl amine, 17 parts of sodium phthalate, 3 parts of 2-carboxybenzaldehyde, 4 parts of di-n-butylamine, 5 parts of maleic acid and 8 parts of ammonium persulfate.
8. the process for tanning of crocodile skin, it is characterised in that crocodile skin is only handled by the following processes carried out successively:
A. soak:Plucked crocodile skin is immersed in the salt solution that PH is 4~5, soak time is 6~8 hours;
B. fleshing:The meat of crocodile skin is rooted out by fleshing machine;
C. soften:Crocodile skin is immersed in the salt solution that PH is 4~5, soak time is 15~20 minutes, then crocodile skin passes through Drain within 4~8 hours;
D. tanning:The raw material of any described tanning agent for crocodile skin of claim 1 to 7 is added in organic solvent, material The weight ratio of liquid is 1:15~25, crocodile skin is immersed in tanning agent solution, soak time is 28~35 hours, and crocodile skin takes out Drained afterwards by 3~4 hours;
E. dry:Crocodile is can obtain after natural drying.
9. the process for tanning of crocodile skin as claimed in claim 8, it is characterised in that:The organic solvent be ethanol, glycerine, It is a kind of or many in isooctane, isopropyl ether, methyl isopropyl ketone, methyltetrahydrofuran, petroleum ether, trichloroacetic acid, trifluoroacetic acid The combination planted.
CN201710452093.5A 2017-06-15 2017-06-15 Tanning agent and its crocodile skin process for tanning for crocodile skin Withdrawn CN107090527A (en)