CN101339363A - Glass decoration picture manufacture method - Google Patents

Glass decoration picture manufacture method Download PDF

Info

Publication number
CN101339363A
CN101339363A CNA2008100456428A CN200810045642A CN101339363A CN 101339363 A CN101339363 A CN 101339363A CN A2008100456428 A CNA2008100456428 A CN A2008100456428A CN 200810045642 A CN200810045642 A CN 200810045642A CN 101339363 A CN101339363 A CN 101339363A
Authority
CN
China
Prior art keywords
printing
minute
half tone
carry out
time
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CNA2008100456428A
Other languages
Chinese (zh)
Inventor
杨伟
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CNA2008100456428A priority Critical patent/CN101339363A/en
Publication of CN101339363A publication Critical patent/CN101339363A/en
Pending legal-status Critical Current

Abstract

The invention discloses a manufacturing method of glass ornamental pictures, sequentially comprising screen stretching, printing down, screen debugging, printing with four-color sensitive ink, printing with false-proof ink, printing with frosted ink, printing with seven-color laser power, printing on tempered glass, and frame manufacturing. The glass ornamental pictures manufactured according to the method of the invention has the advantages of various patterns, long life time, no depigmentation, simple manufacturing method and wide application.

Description

The manufacture method of glass decoration picture
Technical field
The present invention relates to a kind of manufacture method of upholstery, relate generally to a kind of manufacture method of glass decoration picture.
Background technology
In the prior art, glass is more and more favored in interior decoration, and particularly glass decoration picture is widely used in interior decoration.The manufacture method of present glass decoration picture mainly contains engraving, goes up color method; Color method on the burn into; Silk screen print method; The hand drawing method; Spraying process; Paper adherography etc., and all there are many defectives in said method, as pattern dullness, shortage new meaning, glass baseplate is broken easily, rapid wear, can not preserve for a long time, color reduction under the long period situation simultaneously can not be given prominence to the individual character and the bright spot of integral product, a little less than causing the market competitiveness, can not form long-term market share or the like.
Summary of the invention
The objective of the invention is to overcome above-mentioned technological deficiency, a kind of manufacture method of glass decoration picture is provided.Adopt the glass decoration picture pattern of manufacturing of the present invention various, can preserve for a long time, keep long-time color can not weaken simultaneously, manufacture method is simple, widely applicable.
For achieving the above object, the technical solution used in the present invention is:
The manufacture method of glass decoration picture is characterized in that: comprise the net that stretches tight successively; Printing down; The half tone debugging; Four color sensation gloss oil ink prints; The anti-forgery ink printing; The frosted ink printing; Seven color radium-shine powder printings; The tempering printing; Make housing, its concrete steps are;
A, net stretches tight: carry out drawing in the net for three times on pneumatic type stretches tight the net machine making, the net machine that for the first time pneumatic type stretched tight is adjusted to 5-6kg, 15-30 minute pressing time, the net machine that for the second time pneumatic type stretched tight is adjusted to 5.5-6.5kg, and 15-30 minute pressing time, the net machine that for the third time pneumatic type stretched tight is adjusted to 7-7.5kg, 15-30 minute pressing time, brush viscosity gum again and fix,, obtain half tone normal temperature dry 15-30 minute earlier;
B, printing down: under the protection optical condition, the half tone that obtains in the A step carries out gluing, the gluing number of times is that positive and negative evenly are coated with 3-4 time photoresists successively, under 40-50 degree temperature, dried 25-40 minute then, carry out being coated with the second time photoresists after the drying, baking is 25-40 minute under 40-50 degree temperature; After the drying, carry out the printing down exposure, the time shutter is 60-120 second, and the half tone after will exposing dashes with clear water and drenched 2-4 minute, dries 25-40 minute under 40-50 degree temperature again;
C, half tone debugging: the half tone that the B step is obtained is contained on the printing machine, and the distance of half tone and glass basis is 0.5-1cm, and pressure is 5-7kg, and the scraper gradient is 55-75 °;
D, four color sensation gloss oil ink prints: after finishing the C step on the printing machine, print colouring in proper order by black, blue or green, yellow, red four looks, after printing first look, take out glass basis and left standstill 3-5 minute, enter drying tunnel oven dry 10-20 minute again, drying tunnel temperature is 160-190 ℃, by drying tunnel speed be 0.8-1.2 rice/minute, carry out developing water development 3-5 minute then, with clear water washing 3-5 minute, respectively carry out all the other three-colour printings by preceding method in oven dry under the 40-50 ℃ of condition after 15-30 minute; Half tone order number: 350-420 order;
E, anti-forgery ink printing: after finishing the D step on the printing machine, carry out the printing of anti-forgery ink, after finishing printing.Directly enter the drying tunnel oven dry, bake out temperature is the 100-130 degree.Time be 2-3 rice/minute, or under natural temperature from doing half tone order number; The 250-350 order;
F, frosted ink printing: after finishing the E step on the printing machine, carry out the frosted ink printing, directly enter the drying tunnel oven dry, bake out temperature is the 100-130 degree.Time be 2-3 rice/minute, half tone order number: 200-250 order;
G, seven color radium-shine powder printings: after finishing the F step on the printing machine, carry out seven color radium-shine powder printings, after finishing printing, directly advance drying tunnel and dry, temperature is the 100-130 degree, the time be 2-3 rice/minute, half tone order number: 120-200 order;
H, tempering ink printing: finishing on the printing machine after G step gathers, carry out the printing of tempering printing ink white, printing process is: full version printing once, directly enter the drying tunnel oven dry then, bake out temperature is the 100-130 degree, the time be 2-3 rice/minute, half tone order number: 150-250 order;
I, making housing.
After the described frosted ink printing, can also carry out the luminous ink printing, directly enter drying tunnel after the printing and dry, bake out temperature is the 100-130 degree.Time be 2-3 rice/minute.
Behind the described tempering ink printing, can also carry out the fragrant printing ink printing, print request is: half tone order number: 180-250 order; Full version printing or local printing after finishing printing, directly enter drying tunnel and dry.Temperature is the 100-130 degree, also can carry out air dry.Time be 2-3 rice/minute.
The invention has the advantages that:
1, adopts four color sensation gloss oil China inks, make the pattern of product meticulous more clear.Adopt printing earlier.Dry the principle of exposure, duplicating of site is more accurate, and be more perfect again, can reach 99% manifest aspect duplicating in the site, and can not lose, and at the bottom of the scrappage, yield rate can reach more than 98%, and traditional silk screen net-point printing, in half tone manufacturing process, just lost the site of 10%-20%, in printing process, lose the site of 10%-20% once again, and also occur easily scrapping.
2, selected printing-ink belongs to environment-friendly materials, and standard reaches export requirement.Can not pollute home environment, help environment protection health.Selected material is famous oil painting both at home and abroad, landscape painting, abstract painting or the like.Demonstrated fully the crystallization of art with life.
3, the printing ink of six kinds of different process has been merged in the present invention, mainly contains: four color sensation gloss oil China inks, and the water transfer ink, tempering printing ink, anti-forgery ink, wine packing frosting technology printing ink, seven color radium-shine powder printing ink wait the printing ink of six kinds of different process.The present invention can adopt tempered glass as carrier, after dropping from eminence, is not easy brokenly essence, preservation that can be permanent, and the product stereoscopic sensation is stronger, and artistic effect is better.
Embodiment
Embodiment 1:
The manufacture method of glass decoration picture comprises the net that stretches tight successively; Printing down; The half tone debugging; Four color sensation gloss oil ink prints; The anti-forgery ink printing; The frosted ink printing; Seven color radium-shine powder printings; The tempering printing; Make housing, its concrete steps are;
A, net stretches tight: carry out drawing in the net for three times on pneumatic type stretches tight the net machine making, the net machine that for the first time pneumatic type stretched tight is adjusted to 5kg, 15 minutes pressing times, the net machine that for the second time pneumatic type stretched tight is adjusted to 5.5kg, and 15 minutes pressing times, the net machine that for the third time pneumatic type stretched tight is adjusted to 7kg, 15 minutes pressing times, brush viscosity gum again and fix,, obtain half tone normal temperature dry 15 minutes earlier;
B, printing down: under the protection optical condition, the half tone that obtains in the A step carries out gluing, and the gluing number of times is that positive and negative evenly are coated with photoresists successively 3 times, dries 25 minutes under 40 degree temperature then, carry out being coated with the second time photoresists after the drying, baking is 25 minutes under 40 degree temperature; After the drying, carry out the printing down exposure, the time shutter is 60 seconds, and the half tone after will exposing dashes with clear water and drenched 2 minutes, dries 25 minutes under 40 degree temperature again;
C, half tone debugging: the half tone that the B step is obtained is contained on the printing machine, and the distance of half tone and glass basis is 0.5cm, and pressure is 5kg, and the scraper gradient is 55 °;
D, four color sensation gloss oil ink prints: after finishing the C step on the printing machine, print colouring in proper order by black, blue or green, yellow, red four looks, after printing first look, take out glass basis and left standstill 3 minutes, enter drying tunnel oven dry 10 minutes again, drying tunnel temperature is 160 ℃, by drying tunnel speed is 0.8 meter/minute, carries out developing water then and develops 3 minutes, with clear water washing 3 minutes, respectively carry out all the other three-colour printings by preceding method in oven dry under 40 ℃ of conditions after 15 minutes; Half tone order number: 350 orders;
E, anti-forgery ink printing: after finishing the D step on the printing machine, carry out the printing of anti-forgery ink, after finishing printing.Directly enter the drying tunnel oven dry, bake out temperature is 100 degree.Time is 2 meters/minute, or does half tone order number under natural temperature certainly; 250 orders;
F, frosted ink printing: after finishing the E step on the printing machine, carry out the frosted ink printing, directly enter the drying tunnel oven dry, bake out temperature is 100 degree.Time is 2 meters/minute, half tone order number: 200 orders;
G, seven color radium-shine powder printings: after finishing the F step on the printing machine, carry out seven color radium-shine powder printings, after finishing printing, directly advance drying tunnel and dry, temperature is 100 degree, and the time is 2 meters/minute, half tone order number: 120 orders;
H, tempering ink printing: finishing on the printing machine after G step gathers, carry out the printing of tempering printing ink white, printing process is: full version printing once directly enters the drying tunnel oven dry then, and bake out temperature is 100 degree, and the time is 2 meters/minute, half tone order number: 150 orders;
I, making housing.
After the frosted ink printing, can also carry out the luminous ink printing, directly enter drying tunnel after the printing and dry, bake out temperature is 100 degree, the time is 2 meters/minute.Behind the tempering ink printing, can also carry out the fragrant printing ink printing, print request is: half tone order number: 180 orders; Full version printing or local printing after finishing printing, directly enter drying tunnel and dry.Temperature is 100 degree, and the time is 2 meters/minute.Also can carry out air dry.
Embodiment 2:
The manufacture method of glass decoration picture comprises the net that stretches tight successively; Printing down; The half tone debugging; Four color sensation gloss oil ink prints; The anti-forgery ink printing; The frosted ink printing; Seven color radium-shine powder printings; The tempering printing; Make housing, its concrete steps are;
A, net stretches tight: carry out drawing in the net for three times on pneumatic type stretches tight the net machine making, the net machine that for the first time pneumatic type stretched tight is adjusted to 6kg, 30 minutes pressing times, the net machine that for the second time pneumatic type stretched tight is adjusted to 6.5kg, and 30 minutes pressing times, the net machine that for the third time pneumatic type stretched tight is adjusted to 7.5kg, 30 minutes pressing times, brush viscosity gum again and fix,, obtain half tone normal temperature dry 30 minutes earlier;
B, printing down: under the protection optical condition, the half tone that obtains in the A step carries out gluing, and the gluing number of times is that positive and negative evenly are coated with photoresists successively 4 times, dries 40 minutes under 50 degree temperature then, carry out being coated with the second time photoresists after the drying, baking is 40 minutes under 50 degree temperature; After the drying, carry out the printing down exposure, the time shutter is 120 seconds, and the half tone after will exposing dashes with clear water and drenched 4 minutes, dries 40 minutes under 50 degree temperature again;
C, half tone debugging: the half tone that the B step is obtained is contained on the printing machine, and the distance of half tone and glass basis is 1cm, and pressure is 7kg, and the scraper gradient is 75 °;
D, four color sensation gloss oil ink prints: after finishing the C step on the printing machine, print colouring in proper order by black, blue or green, yellow, red four looks, after printing first look, take out glass basis and left standstill 5 minutes, enter drying tunnel oven dry 20 minutes again, drying tunnel temperature is 190 ℃, by drying tunnel speed is 1.2 meters/minute, carries out developing water then and develops 5 minutes, with clear water washing 5 minutes, respectively carry out all the other three-colour printings by preceding method in oven dry under 50 ℃ of conditions after 30 minutes; Half tone order number: 420 orders;
E, anti-forgery ink printing: after finishing the D step on the printing machine, carry out the printing of anti-forgery ink, after finishing printing.Directly enter the drying tunnel oven dry, bake out temperature is 130 degree.Time is 3 meters/minute, or does half tone order number under natural temperature certainly; 350 orders;
F, frosted ink printing: after finishing the E step on the printing machine, carry out the frosted ink printing, directly enter the drying tunnel oven dry, bake out temperature is 130 degree.Time is 3 meters/minute, half tone order number: 250 orders;
G, seven color radium-shine powder printings: after finishing the F step on the printing machine, carry out seven color radium-shine powder printings, after finishing printing, directly advance drying tunnel and dry, temperature is 130 degree, and the time is 3 meters/minute, half tone order number: 200 orders;
H, tempering ink printing: finishing on the printing machine after G step gathers, carry out the printing of tempering printing ink white, printing process is: full version printing once directly enters the drying tunnel oven dry then, and bake out temperature is 130 degree, and the time is 3 meters/minute, half tone order number: 250 orders;
I, making housing.
After the frosted ink printing, can also carry out the luminous ink printing, directly enter drying tunnel after the printing and dry, bake out temperature is 130 degree.Time is 3 meters/minute.Behind the tempering ink printing, can also carry out the fragrant printing ink printing, print request is: half tone order number: 250 orders; Full version printing or local printing after finishing printing, directly enter drying tunnel and dry.Temperature is 130 degree, and the time is 3 meters/minute.Also can carry out air dry.
Embodiment 3:
The manufacture method of glass decoration picture comprises the net that stretches tight successively; Printing down; The half tone debugging; Four color sensation gloss oil ink prints; The anti-forgery ink printing; The frosted ink printing; Seven color radium-shine powder printings; The tempering printing; Make housing, its concrete steps are;
A, net stretches tight: carry out drawing in the net for three times on pneumatic type stretches tight the net machine making, the net machine that for the first time pneumatic type stretched tight is adjusted to 5.5kg, 25 minutes pressing times, the net machine that for the second time pneumatic type stretched tight is adjusted to 6kg, and 25 minutes pressing times, the net machine that for the third time pneumatic type stretched tight is adjusted to 7.5kg, 25 minutes pressing times, brush viscosity gum again and fix,, obtain half tone normal temperature dry 25 minutes earlier;
B, printing down: under the protection optical condition, the half tone that obtains in the A step carries out gluing, and the gluing number of times is that positive and negative evenly are coated with photoresists successively 4 times, dries 35 minutes under 45 degree temperature then, carry out being coated with the second time photoresists after the drying, baking is 35 minutes under 45 degree temperature; After the drying, carry out the printing down exposure, the time shutter is 80 seconds, and the half tone after will exposing dashes with clear water and drenched 3 minutes, dries 35 minutes under 45 degree temperature again;
C, half tone debugging: the half tone that the B step is obtained is contained on the printing machine, and the distance of half tone and glass basis is 0.7cm, and pressure is 6kg, and the scraper gradient is 65 °;
D, four color sensation gloss oil ink prints: after finishing the C step on the printing machine, print colouring in proper order by black, blue or green, yellow, red four looks, after printing first look, take out glass basis and left standstill 4 minutes, enter drying tunnel oven dry 15 minutes again, drying tunnel temperature is 170 ℃, by drying tunnel speed is 1 meter/minute, carries out developing water then and develops 4 minutes, with clear water washing 4 minutes, respectively carry out all the other three-colour printings by preceding method in oven dry under 45 ℃ of conditions after 25 minutes; Half tone order number: 400 orders;
E, anti-forgery ink printing: after finishing the D step on the printing machine, carry out the printing of anti-forgery ink, after finishing printing.Directly enter the drying tunnel oven dry, bake out temperature is 110 degree.Time is 2.5 meters/minute, or does half tone order number under natural temperature certainly; 300 orders;
F, frosted ink printing: after finishing the E step on the printing machine, carry out the frosted ink printing, directly enter the drying tunnel oven dry, bake out temperature is 110 degree.Time is 2.5 meters/minute, half tone order number: 225 orders;
G, seven color radium-shine powder printings: after finishing the F step on the printing machine, carry out seven color radium-shine powder printings, after finishing printing, directly advance drying tunnel and dry, temperature is 110 degree, and the time is 2.5 meters/minute, half tone order number: 180 orders;
H, tempering ink printing: finishing on the printing machine after G step gathers, carry out the printing of tempering printing ink white, printing process is: full version printing once directly enters the drying tunnel oven dry then, and bake out temperature is 110 degree, and the time is 2.5 meters/minute, half tone order number: 200 orders;
I, making housing.
After the frosted ink printing, can also carry out the luminous ink printing, directly enter drying tunnel after the printing and dry, bake out temperature is 110 degree, the time is 2.5 meters/minute.Behind the tempering ink printing, can also carry out the fragrant printing ink printing, print request is: half tone order number: 200 orders; Full version printing or local printing after finishing printing, directly enter drying tunnel and dry.Temperature is 110 degree, and the time is 2.5 meters/minute.Also can carry out air dry.
Embodiment 4:
The manufacture method of glass decoration picture comprises the net that stretches tight successively; Printing down; The half tone debugging; Four color sensation gloss oil ink prints; The anti-forgery ink printing; The frosted ink printing; Seven color radium-shine powder printings; The tempering printing; Make housing, its concrete steps are;
A, net stretches tight: carry out drawing in the net for three times on pneumatic type stretches tight the net machine making, the net machine that for the first time pneumatic type stretched tight is adjusted to 5kg, 30 minutes pressing times, the net machine that for the second time pneumatic type stretched tight is adjusted to 5.5kg, and 30 minutes pressing times, the net machine that for the third time pneumatic type stretched tight is adjusted to 7kg, 30 minutes pressing times, brush viscosity gum again and fix,, obtain half tone normal temperature dry 15 minutes earlier;
B, printing down: under the protection optical condition, the half tone that obtains in the A step carries out gluing, and the gluing number of times is that positive and negative evenly are coated with photoresists successively 3 times, dries 25 minutes under 50 degree temperature then, carry out being coated with the second time photoresists after the drying, baking is 25 minutes under 50 degree temperature; After the drying, carry out the printing down exposure, the time shutter is 120 seconds, and the half tone after will exposing dashes with clear water and drenched 2 minutes, dries 25 minutes under 50 degree temperature again;
C, half tone debugging: the half tone that the B step is obtained is contained on the printing machine, and the distance of half tone and glass basis is 1cm, and pressure is 5kg, and the scraper gradient is 75 °;
D, four color sensation gloss oil ink prints: after finishing the C step on the printing machine, print colouring in proper order by black, blue or green, yellow, red four looks, after printing first look, take out glass basis and left standstill 3 minutes, enter drying tunnel oven dry 20 minutes again, drying tunnel temperature is 160 ℃, by drying tunnel speed is 1.2 meters/minute, carries out developing water then and develops 3 minutes, with clear water washing 5 minutes, respectively carry out all the other three-colour printings by preceding method in oven dry under 40 ℃ of conditions after 30 minutes; Half tone order number: 350 orders;
E, anti-forgery ink printing: after finishing the D step on the printing machine, carry out the printing of anti-forgery ink, after finishing printing.Directly enter the drying tunnel oven dry, bake out temperature is 130 degree.Time is 2 meters/minute, or does half tone order number under natural temperature certainly; 350 orders;
F, frosted ink printing: after finishing the E step on the printing machine, carry out the frosted ink printing, directly enter the drying tunnel oven dry, bake out temperature is 100 degree.Time is 3 meters/minute, half tone order number: 200 orders;
G, seven color radium-shine powder printings: after finishing the F step on the printing machine, carry out seven color radium-shine powder printings, after finishing printing, directly advance drying tunnel and dry, temperature is 130 degree, and the time is 2 meters/minute, half tone order number: 200 orders;
H, tempering ink printing: finishing on the printing machine after G step gathers, carry out the printing of tempering printing ink white, printing process is: full version printing once directly enters the drying tunnel oven dry then, and bake out temperature is 130 degree, and the time is 2 meters/minute, half tone order number: 250 orders;
I, making housing.
After the frosted ink printing, can also carry out the luminous ink printing, directly enter drying tunnel after the printing and dry, bake out temperature is 130 degree, the time is 2 meters/minute.Behind the tempering ink printing, can also carry out the fragrant printing ink printing, print request is: half tone order number: 250 orders; Full version printing or local printing after finishing printing, directly enter drying tunnel and dry.Temperature is 130 degree, and the time is 2 meters/minute.Also can carry out air dry.
Embodiment 5:
The manufacture method of glass decoration picture comprises the net that stretches tight successively; Printing down; The half tone debugging; Four color sensation gloss oil ink prints; The anti-forgery ink printing; The frosted ink printing; Seven color radium-shine powder printings; The tempering printing; Make housing, its concrete steps are;
A, net stretches tight: carry out drawing in the net for three times on pneumatic type stretches tight the net machine making, the net machine that for the first time pneumatic type stretched tight is adjusted to 6.2kg, 31 minutes pressing times, the net machine that for the second time pneumatic type stretched tight is adjusted to 6.3kg, and 28 minutes pressing times, the net machine that for the third time pneumatic type stretched tight is adjusted to 7.1kg, 20 minutes pressing times, brush viscosity gum again and fix,, obtain half tone normal temperature dry 22 minutes earlier;
B, printing down: under the protection optical condition, the half tone that obtains in the A step carries out gluing, and the gluing number of times is that positive and negative evenly are coated with photoresists successively 3 times, dries 38 minutes under 42 degree temperature then, carry out being coated with the second time photoresists after the drying, baking is 30 minutes under 42 degree temperature; After the drying, carry out the printing down exposure, the time shutter is 90 seconds, and the half tone after will exposing dashes with clear water and drenched 3 minutes, dries 30 minutes under 42 degree temperature again;
C, half tone debugging: the half tone that the B step is obtained is contained on the printing machine, and the distance of half tone and glass basis is 0.8cm, and pressure is 6kg, and the scraper gradient is 60 °;
D, four color sensation gloss oil ink prints: after finishing the C step on the printing machine, print colouring in proper order by black, blue or green, yellow, red four looks, after printing first look, take out glass basis and left standstill 4 minutes, enter drying tunnel oven dry 15 minutes again, drying tunnel temperature is 170 ℃, by drying tunnel speed is 0.9 meter/minute, carries out developing water then and develops 4 minutes, with clear water washing 4 minutes, respectively carry out all the other three-colour printings by preceding method in oven dry under 48 ℃ of conditions after 28 minutes; Half tone order number: 400 orders;
E, anti-forgery ink printing: after finishing the D step on the printing machine, carry out the printing of anti-forgery ink, after finishing printing.Directly enter the drying tunnel oven dry, bake out temperature is 120 degree.Time is 2.5 meters/minute, or does half tone order number under natural temperature certainly; 300 orders;
F, frosted ink printing: after finishing the E step on the printing machine, carry out the frosted ink printing, directly enter the drying tunnel oven dry, bake out temperature is 120 degree.Time is 2.5 meters/minute, half tone order number: 200 orders;
G, seven color radium-shine powder printings: after finishing the F step on the printing machine, carry out seven color radium-shine powder printings, after finishing printing, directly advance drying tunnel and dry, temperature is 120 degree, and the time is 2.5 meters/minute, half tone order number: 180 orders;
H, tempering ink printing: finishing on the printing machine after G step gathers, carry out the printing of tempering printing ink white, printing process is: full version printing once directly enters the drying tunnel oven dry then, and bake out temperature is 120 degree, and the time is 2.5 meters/minute, half tone order number: 200 orders;
I, making housing.
After the frosted ink printing, can also carry out the luminous ink printing, directly enter drying tunnel after the printing and dry, bake out temperature is 120 degree.Time is 2.5 meters/minute.Behind the tempering ink printing, can also carry out the fragrant printing ink printing, print request is: half tone order number: 200 orders; Full version printing or local printing after finishing printing, directly enter drying tunnel and dry.Temperature be 120 the degree, the time be 2-3 rice/minute.Also can carry out air dry.

Claims (3)

1, the manufacture method of glass decoration picture is characterized in that: comprise the net that stretches tight successively; Printing down;
The half tone debugging; Four color sensation gloss oil ink prints; The anti-forgery ink printing; The frosted ink printing; Seven color radium-shine powder printings; The tempering printing; Make housing, its concrete steps are;
A, net stretches tight: carry out drawing in the net for three times on pneumatic type stretches tight the net machine making, the net machine that for the first time pneumatic type stretched tight is adjusted to 5-6kg, 15-30 minute pressing time, the net machine that for the second time pneumatic type stretched tight is adjusted to 5.5-6.5kg, and 15-30 minute pressing time, the net machine that for the third time pneumatic type stretched tight is adjusted to 7-7.5kg, 15-30 minute pressing time, brush viscosity gum again and fix,, obtain half tone normal temperature dry 15-30 minute earlier;
B, printing down: under the protection optical condition, the half tone that obtains in the A step carries out gluing, the gluing number of times is that positive and negative evenly are coated with 3-4 time photoresists successively, under 40-50 degree temperature, dried 25-40 minute then, carry out being coated with the second time photoresists after the drying, baking is 25-40 minute under 40-50 degree temperature; After the drying, carry out the printing down exposure, the time shutter is 60-120 second, and the half tone after will exposing dashes with clear water and drenched 2-4 minute, dries 25-40 minute under 40-50 degree temperature again;
C, half tone debugging: the half tone that the B step is obtained is contained on the printing machine, and the distance of half tone and glass basis is 0.5-1cm, and pressure is 5-7kg, and the scraper gradient is 55-75 °;
D, four color sensation gloss oil ink prints: after finishing the C step on the printing machine, print colouring in proper order by black, blue or green, yellow, red four looks, after printing first look, take out glass basis and left standstill 3-5 minute, enter drying tunnel oven dry 10-20 minute again, drying tunnel temperature is 160-190 ℃, by drying tunnel speed be 0.8-1.2 rice/minute, carry out developing water development 3-5 minute then, with clear water washing 3-5 minute, respectively carry out all the other three-colour printings by preceding method in oven dry under the 40-50 ℃ of condition after 15-30 minute; Half tone order number: 350-420 order;
E, anti-forgery ink printing: after finishing the D step on the printing machine, carry out the printing of anti-forgery ink, after finishing printing.Directly enter the drying tunnel oven dry, bake out temperature is the 100-130 degree.Time be 2-3 rice/minute, or under natural temperature from doing half tone order number; The 250-350 order;
F, frosted ink printing: after finishing the E step on the printing machine, carry out the frosted ink printing, directly enter the drying tunnel oven dry, bake out temperature is the 100-130 degree.Time be 2-3 rice/minute, half tone order number: 200-250 order;
G, seven color radium-shine powder printings: after finishing the F step on the printing machine, carry out seven color radium-shine powder printings, after finishing printing, directly advance drying tunnel and dry, temperature is the 100-130 degree, the time be 2-3 rice/minute, half tone order number: 120-200 order;
H, tempering ink printing: finishing on the printing machine after G step gathers, carry out the printing of tempering printing ink white, printing process is: full version printing once, directly enter the drying tunnel oven dry then, bake out temperature is the 100-130 degree, the time be 2-3 rice/minute, half tone order number: 150-250 order;
I, making housing.
2, the manufacture method of glass decoration picture according to claim 1 is characterized in that: after the described frosted ink printing, can also carry out the luminous ink printing, directly enter drying tunnel after the printing and dry, bake out temperature is the 100-130 degree.Time be 2-3 rice/minute.
3, the manufacture method of glass decoration picture according to claim 1 and 2, it is characterized in that: behind the described tempering ink printing, can also carry out the fragrant printing ink printing, print request is: half tone order number: the 180-250 order, and full version printing or local printing are after finishing printing, directly entering drying tunnel dries, temperature is the 100-130 degree, the time be 2-3 rice/minute, also can carry out air dry.
CNA2008100456428A 2008-07-25 2008-07-25 Glass decoration picture manufacture method Pending CN101339363A (en)