CN100425392C - 高硅钢薄板的冷轧制备方法 - Google Patents

高硅钢薄板的冷轧制备方法 Download PDF

Info

Publication number
CN100425392C
CN100425392C CNB2007100991305A CN200710099130A CN100425392C CN 100425392 C CN100425392 C CN 100425392C CN B2007100991305 A CNB2007100991305 A CN B2007100991305A CN 200710099130 A CN200710099130 A CN 200710099130A CN 100425392 C CN100425392 C CN 100425392C
Authority
CN
China
Prior art keywords
rolling
cold rolling
plate
warm
hot
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CNB2007100991305A
Other languages
English (en)
Other versions
CN101049669A (zh
Inventor
林均品
梁永锋
叶丰
王艳丽
陈国良
张勇
林志
刘艳
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
University of Science and Technology Beijing USTB
Original Assignee
University of Science and Technology Beijing USTB
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by University of Science and Technology Beijing USTB filed Critical University of Science and Technology Beijing USTB
Priority to CNB2007100991305A priority Critical patent/CN100425392C/zh
Publication of CN101049669A publication Critical patent/CN101049669A/zh
Application granted granted Critical
Publication of CN100425392C publication Critical patent/CN100425392C/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

一种高硅钢薄板的冷轧制备方法,属于金属材料制备技术领域。薄板中Fe含量为85-96%,Si含量为4-15%,均为重量比;其工艺为:原料准备:硅含量的范围为4-15%,硼的含量为100-5000ppm,其余为铁;冶炼,浇铸;锻造成厚度10-20mm的板坯;热轧到1-2mm;热轧板热处理;温轧得到0.2-0.3mm的板材;温轧板热处理;冷轧得到厚度为0.03-0.05mm的高硅钢板。优点在于,利用冷轧方法制备该合金,而由于该材料的室温脆性,该传统方法在之前被认为不可能制备出高硅钢。所制备出来的冷轧薄带具有良好的板形,表面具有金属光泽。该生产工艺具有普遍适用性,成本低;由于高硅钢优异的软磁性能,具有广阔的市场应用前景。

Description

高硅钢薄板的冷轧制备方法
技术领域
本发明属于金属材料制备技术领域,涉及一种含硼高硅钢的冷轧制备方法。
技术背景
硅钢是使用量最大的一类软磁合金,含硅量一般为1.5~3.5%(重量比,下同)。是电力和电讯工业用以制造发电机、电动机、变压器、互感器、继电器以及其它电器仪表的重要磁性材料。
高硅钢一般指含硅量超过3.5%的硅钢。随着硅含量的增加,硅钢的软磁性能提高,表现在电阻率和磁导率的增加,矫顽力和磁晶各向异性能的降低。在6.5%硅含量时,硅钢性能表现最优。1928年Schulze发现Fe-6.5%Si合金的磁滞伸缩常数(λ,)接近于零。1942年Ruder指出,和Fe-3.5%Si合金相比,Fe-6.5%Si合金的磁晶各向异性常数KI和磁致伸缩常数λs更低,电阻率ρ更高,所以铁损P更低。1964年Brown等证明Fe-6.5%Si单晶体比Fe-3.5%Si单晶体的P15/50低0.2W/kg,λs低90%,KI低1/3。因而与普通硅钢相比,高硅钢具有优异的磁性能,可以得到低的铁损和小的磁致伸缩,对节约能源,降低噪音有着重要的作用。
但随着Si含量的增加,铁硅合金的加工性能变差,4.0%Si一般为硅钢制品的上限。超过此范围,合金中出现铁硅的有序相,大大提高了材料的脆性,因而难于用传统的轧制方法生产高硅钢板。由于高硅钢有严重的脆性,各发达国家相继采用特殊的工艺制备该合金薄板。Y.Takada在Journal of Applied Physics,64(10):5367-5369,1988,Commercial scale production of Fe-6.5wt.% Si sheet and its magneticproperties中提到用CVD(Chemical Vapor Deposition)方法生产此合金。该工艺包括两个步骤,第一步先将普通硅钢轧到一定厚度,第二步对此钢板进行化学气象沉积,在表面沉积硅,然后进行扩散退火。该工艺虽然已基本成熟,但生产工艺复杂,生产周期长,生产成本高,且所用原料SiCl4对环境有污染。G.E.Fish等在Journal of Applied Physics,64(10):5370,1988,Frequency dependence ofcore loss inrapidly quenched Fe-6.5wt.%Si中报道用快速凝固法制备该合金薄带。其特点是直接由液态合金甩带,避开其脆性区,直接得到薄而窄的合金薄带。但所得薄带尺寸受限制,因而不利于大规模生产和应用。T.Ros-Yanez等在Journal of MaterialsProcessing Technology,143-144:916-921,2003,Production of high silicon steel forelectrical application by thermomechanical processing中报道,用传统的热轧冷轧方法制备该合金。但冷轧之前,须调整轧制方向,沿热轧方向旋转90°,即沿热轧板的横向进行冷轧,因而这种工艺也不适合大批量生产此合金。
发明内容
本发明的目的在于提供一种高硅钢薄板的冷轧制备方法,对于含硅4~15%的高硅钢,利用锻造,热轧,温轧,冷轧法,结合相应的热处理工艺,制备0.03~0.05mm薄带。薄带具有良好的板形,表面具有金属光泽。该生产工艺具有普遍适用性,可以在传统的轧机上进行,不需要对现有设备进行大的改造。同时冷轧方向与热轧方向相同,因而热轧板可以沿轧制方向继续冷轧,保持了板带材的连续性。
具体的工艺流程(参见图1)为:
(1)原料准备:以工业纯铁(工业纯铁DTO,铁含量99.5%)、晶体硅(纯度为99.9%)、硼铁(含硼20.43%)为原料,按硅含量4~15%,硼含量100~5000ppm的比例进行配比混合;
(2)冶炼:用中频真空感应炉熔炼原料纯铁、硅和硼铁,1300~1530℃浇铸;
(3)锻造:采用空气锤自由煅,在1250℃~750℃将铸锭锻造成厚度为10~20mm的板坯,锻造不仅可以提供适宜于热轧的原料形状,而且可以破碎晶粒和夹杂物,提高材料的塑性;
(4)热轧:1250~500℃热轧到1~2mm,在此过程中材料发生较大变形,同时发生动态再结晶,晶粒细化;
(5)热轧板热处理:在700~1000℃保温1~3小时后水或盐水中冷却。热处理使材料发生回复和再结晶,消除加工硬化,并且快速冷却降低了材料的有序度。
(6)温轧:在700~150℃温轧,得到0.2~0.3mm的板材。在再结晶温度以下轧制,获得纤维状轧制组织,增加材料塑性。
(7)温轧板热处理:在700~1000℃保温1~3小时后水或盐水中冷却。此热处理在保护气氛下进行,防止板材表面氧化,影响后续冷轧加工。此热处理消除了加工硬化,快速冷却降低了材料的有序度;
(8)冷轧:室温下冷轧,第一道次压下量为20~70%,第二道次压下量为10~50%,之后反复冷轧,直至厚度达到0.03~0.05mm。经过冷轧,得到极薄板材,并且板材板形整齐,表面质量好,具有金属光泽。
本发明的温轧板热处理在保护气氛中进行,采用氩气或氮气下进行。
本发明的冷轧第一道次压下量为20~70%,第二道次压下量为10~50%,之后反复冷轧,直至厚度达到0.03~0.05mm。
本发明的优点在于:
本发明提出用传统的轧制方法制备高硅钢的技术。而由于该材料的室温脆性,该传统方法在之前被认为不可能制备出高硅钢。因而利用此方法,可以利用传统的锻造机和轧钢机制备该合金薄板,具有广泛的适用性。并且所用原材料简单,纯度不高,具有成本低的优点。
高硅钢中存在铁硅的有序相,对材料的塑性影响很大,同时材料中所含非金属杂质,如碳、氧、氮等对该材料的磁性能影响较大,因而从制备工艺的各个环节着手,一方面降低铁硅有序相的含量,提高塑性,另一方面减少杂质含量,提高合金的磁性能。
冶炼时采取真空感应炉熔炼,可以降低杂质含量,提高合金塑性及磁性能。硼元素的加入,能够细化铸造组织晶粒,保证锻造的顺利进行。锻造和热轧过程,能够提供较薄的板材,并且细化晶粒。温轧过程是实现冷轧的关键步骤,在再结晶温度以下的温轧,能够得到拉长的纤维组织,提高材料的塑性。冷轧时第一、第二道次采用较大的压下量,使原子站位发生激烈重组,促进有序合金的无序化,同时利用大变形过程当中的变形热,使材料温度升高,冷轧能够顺利进行。而在此制备过程当中所采取的合适的热处理制度,不仅能够使材料发生回复再结晶,消除加工硬化,提高塑性,更能使合金从无序状态急冷,降低合金的有序度,大大地提高了塑性。
本发明从原料控制、工艺路线着手研究,能够节约成本,具有现实的推广应用价值,具有其他制备方法无可比拟的优势,同时由于此种高硅钢具有优异的软磁性能,因而具有广阔的市场应用前景。
附图说明
图1为本发明的制备工艺流程图。
图2为本发明的温轧0.3mm薄板。
图3为本发明的冷轧0.05mm薄板,
图4为本发明的薄带的弯曲实验。
具体实施方式
对于硅含量在4~15%,硼含量在100~5000ppm的高硅钢,利用轧制的方法,制备薄板,具体的实施方案如下:
实施例1
对于含硅4.5%,含硼200ppm的高硅钢,用中频真空感应炉熔炼原料,浇铸温度1530℃。铸锭随后进行自由锻造,初锻温度1200℃,终锻温度900℃,铸锭采取随炉升温的方式,以防止热应力产生裂纹。
锻造后板坯厚20mm,随后进行热轧,热轧开轧温度1200℃,终轧温度700℃。板坯热轧至1.5mm。所得热轧板经过热处理,热处理温度为900℃,保温时间1h,水冷却。
处理后的热轧板酸洗之后,进行温轧,开轧温度500℃,终轧温度150℃,压下量为每道次30%,得到0.3mm温轧板。
温轧板经过900℃,1h保温处理,水冷却,表面经过处理后进行冷轧。冷轧第一道次40%,第二道次30%,随后不断减小辊缝,反复冷轧至0.05mm。
实施例2
对于含硅5.8%,含硼600ppm的高硅钢,用中频真空感应炉熔炼原料,浇铸温度1500℃。铸锭随后进行自由锻造,始锻温度1200℃,终锻温度850℃,铸锭采取随炉升温的方式,以防止热应力产生裂纹。
锻造后得到板坯厚20mm,随后进行热轧,热轧开轧温度1200℃,终轧温度650℃,板坯热轧至1.5mm。所得热轧板经过热处理,热处理温度为900℃,保温时间2h,水冷却。
处理后的热轧板酸洗之后,进行温轧。开轧温度650℃,终轧温度200℃温度,压下量为每道次25%,得到0.3mm温轧板。
温轧板经过850℃,1h保温处理,水冷却,表面经过处理后进行冷轧。冷轧第一道次35%,第二道次30%,随后不断减小辊缝,反复冷轧至0.03mm。
实施例3
对于含硅6.5%,含硼1000ppm的高硅钢,用中频真空感应炉熔炼原料,浇铸温度1480℃。铸锭随后进行自由锻造,开锻温度1100℃,终锻温度850℃,锻造的铸锭采取随炉升温的方式,以防止热应力产生裂纹。
锻造后得到板坯厚20mm,随后进行热轧,热轧开轧温度1150℃,终轧温度650℃。板坯热轧至1mm。所得热轧板经过热处理,热处理温度为900℃,保温时间2h,盐水冷却。
处理后的热轧板酸洗之后,进行温轧。开轧温度650℃,终轧温度250℃,压下量为每道次25%,得到0.3mm温轧板。温轧板经过900℃,1h保温处理,盐水冷却,表面经过处理后进行冷轧。
冷轧第一道次40%,第二道次30%,随后不断减小辊缝,反复冷轧至0.03mm。
实施例4
对于含硅7.5%,含硼2000ppm的高硅钢,用中频真空感应炉熔炼原料,浇铸温度1460℃。铸锭随后进行自由锻造,开锻温度1100℃,终锻温度800℃。铸锭采取随炉升温的方式,以防止热应力产生裂纹。
锻造后得到板坯厚15mm,随后进行热轧,热轧开轧温度1100℃,终轧温度700℃,板坯热轧至1mm。所得热轧板经过热处理,热处理温度为900℃,保温时间3h,盐水冷却。
处理后的热轧板酸洗之后,进行温轧。开轧温度700℃,终轧温度300℃,压下量为每道次25%,得到0.3mm温轧板。温轧板经过900℃,2h保温处理,盐水冷却,表面经过处理后进行冷轧。
冷轧第一道次45%,第二道次30%,随后不断减小辊缝,反复冷轧至0.05mm。
实施例5
对于含硅12%,含硼4000ppm的高硅钢,用中频真空感应炉熔炼原料,浇铸温度1400℃。铸锭随后进行自由锻造,开锻温度1050℃,终锻温度800℃,锻造的铸锭采取随炉升温的方式,以防止热应力产生裂纹。
锻造后得到板坯厚15mm,随后进行热轧,热轧开轧温度1000℃,终轧温度700℃,板坯热轧至1mm。所得热轧板经过热处理,热处理温度为900℃,保温时间3h,盐水冷却。
处理后的热轧板酸洗之后,进行温轧。开轧温度700℃,终轧温度400℃,压下量为每道次25%,得到0.3mm温轧板。温轧板经过900℃,2h保温处理,盐水冷却,表面经过处理后进行冷轧。
冷轧第一道次50%,第二道次35%,随后不断减小辊缝,反复冷轧至0.05mm。

Claims (3)

1.一种高硅钢薄板的冷轧制备方法,薄板中Fe含量为85~96%,Si含量为4~15%,均为重量百分比;其工艺为:
(1)原料准备:工业纯铁、晶体硅、硼铁为原料,要得到的硅含量的范围为4~15%,硼的含量为100~5000ppm,其余为铁;
(2)冶炼:用中频真空感应炉熔炼原料纯铁、硅和硼铁,1300~1530℃浇铸;
(3)锻造:在1250℃~750℃锻造成厚度10~20mm的板坯;
(4)热轧:1250~500℃热轧到1~2mm;
(5)热轧板退火:在700~1000℃保温1~3小时后水或盐水中冷却;
(6)温轧:在700~150℃温轧,得到0.2~0.3mm的板材;
(7)温轧板热处理:在700~1000℃保温1~3小时后水或盐水中冷却;
(8)冷轧:室温下冷轧,得到厚度为0.03~0.05mm的高硅钢板;
2.根据权利要求1所述的高硅钢薄板的冷轧制备方法,其特征是,温轧板热处理在保护气氛中进行,采用氩气或氮气下进行。
3.根据权利要求1所述的高硅钢薄板的冷轧制备方法,冷轧第一道次压下量为20~70%,第二道次压下量为10~50%,之后反复冷轧,直至厚度达到0.03~0.05mm。
CNB2007100991305A 2007-05-14 2007-05-14 高硅钢薄板的冷轧制备方法 Expired - Fee Related CN100425392C (zh)