WO2005084845A1 - An article made of a magnesium alloy tube - Google Patents

An article made of a magnesium alloy tube Download PDF

Info

Publication number
WO2005084845A1
WO2005084845A1 PCT/IL2005/000246 IL2005000246W WO2005084845A1 WO 2005084845 A1 WO2005084845 A1 WO 2005084845A1 IL 2005000246 W IL2005000246 W IL 2005000246W WO 2005084845 A1 WO2005084845 A1 WO 2005084845A1
Authority
WO
WIPO (PCT)
Prior art keywords
tube
extrusion
temperature
predetermined
sec
Prior art date
Application number
PCT/IL2005/000246
Other languages
French (fr)
Inventor
Eli Spinat
Stefan Jaeger
Adi Ben-Artzy
Original Assignee
Magtech-Magnesium Technologies Ltd.
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Magtech-Magnesium Technologies Ltd. filed Critical Magtech-Magnesium Technologies Ltd.
Priority to DE112005000491T priority Critical patent/DE112005000491T5/en
Priority to US10/591,125 priority patent/US20070181235A1/en
Publication of WO2005084845A1 publication Critical patent/WO2005084845A1/en

Abstract

An article made of a magnesium alloy tube (23) is provided, the article having a grain size of between 10µm and 50µm and being manufactured by internal high pressure forming. The temperature of the internal high pressure forming is between 200°C and 605°C. The tube (23) is manufactured by extrusion, wherein the extrusion temperature is between 300°C and 605°C, the extrusion speed is substantially between 5 mm/sec and 45 mm/sec, and the extrusion reduction ratio is substantially between 10:1 and 50:1. The tube (23) may be annealed for 6 hours at 300°C

Description

AN ARTICLE MADE OF A MAGNESIUM ALLOY TUBE
FIELD OF THE INVENTION This invention relates to processes for extrusion of tubes from metal alloys and structures formed by such processes, in particular to extrusion, using magnesium alloys.
BACKGROUND OF THE INVENTION Metal profiles and tubes are often produced using extrusion. In the process, a round metal block called a "billet" is introduced into a heated container, having a ram at one end and a die at the other. The ram is used to apply a pressure; on the billet in the direction of the die. The billet is forced through an aperture in "the die, and the metal undergoes a deformation into an extruded body, having a cross- section in the shape of the aperture. This is referred to as direct extrusion. In another known method of extrusion, the die is moved toward the billet. Trie billet therefore is stationary with respect to the container, eliminating friction there and reducing the pressure needed for extrusion. However, surface defects on t ie billet are propagated to the extruded material. This is referred to indirect extrusion - The deformation of an object with one cross-sectional area into an o~ϊ ject of a smaller cross-sectional area results in an increase in length. The ratio of the cross- sectional area of the billet to the cross-sectional area of the extruded body is referred to in the art as well as in the present specification and claims., as the extrusion reduction ratio. In order to create hollow shapes such as tubes using extrusion, a mandrel is placed inside the die aperture. The metal is forced to flow between the die and the mandrel, causing a hollow having the shape of the mandrel to be formed in the metal. Recently, internal high pressure forming (IHPF) has been utilized to form parts having complex geometries, particularly in the automotive industry. IHPF utilizes fluid pressure to form the part into the desired shape of a mold. Using this process, components that would otherwise be manufactured as several pieces and then joined together can be manufactured as one. This reduces the mass of the component and maintains its stifmess, due to the elimination of spot-welded joints. Other advantages of using IHPF include weight reduction through more efficient section design of the component and tailoring of its wall thickness, improved structural strength, lower tooling cost due to fewer parts, fewer secondary operations such as welding of sections, tighter dimensional tolerances, and fewer parts required for final assembly. Presently, IHPF is used to manufacture steel and aluminium parts.
SUMMARY OF THE INVENTION The present invention is directed toward adaptation of internal high pressure forming to magnesium, for use, in particular, in reducing a vehicle's weight and to thereby increase fuel economy and reduce emissions. According to one aspect of the present invention, there is provided an article made of a magnesium alloy tube, the article having a grain size of between lOμm and 50μm and being manufactured by internal high pressure forming. The temperature of the internal high pressure forming is between 200°C and 605°C. The tube is manufactured by extrusion, wherein the extrusion temperature is between 300°C and 605°C, the extrusion speed is substantially between 5 mm/sec and 45 mm/sec, and the extrusion reduction ratio is substantially between 10:1 and 50:1. The tube may be annealed for 6 hours at 300°C. According to another aspect of the present invention, there is provided a process for forming a hollow tube by extrusion of a billet made from a magnesium alloy, comprising the steps of heating the billet to a predetermined temperature within a temperature range, extruding the billet using an indirect extrusion process, wherein the temperature is within a range of 300°C to 605°C, the extrusion speed is substantially in the range between 5 mm/sec and 45 mm/sec, and the extrusion reduction ratio is substantially in the range between 10:1 and 50:1. According to a further aspect of the invention, there is provided a process for internal high pressure forming using tubes obtained according to the above- described process. The process comprises the steps of cooling the tube in a predetermined temperature for a predetermined amount of time, sealing the tube from both ends, introducing a pressure medium into the tube, positioning the tube in a mold having a guiding zone and an expansion zone, wherein the temperature of the expansion zone is between 200°C and 605°C, and applying an axial compression force on the tube, the result being that the portion of the tube that is within the expansion zone expands to fill the zone and adopt thereby its shape. The tube is then cooled for a predetermined period of time at a predetermined temperature.
BRIEF DESCRIPTION OF THE DRAWINGS In order to understand the invention and to see how it may be carried out in practice, an embodiment will now be described, by way of non-limiting example only, with reference to the accompanying drawings, in which: Fig. 1 shows a partial cut-away view of a typical extrusion press which may be used with an extrusion process of the present invention; Fig. 2 is an illustration of a typical setup for a tooling which may be used in internal high pressure forming; and Fig. 3 is an illustration the setup of Fig. 2, wherein a tube is undergoing internal high pressure forming. DETAILED DESCRIPTION OF THE INVENTION An extrusion press, known in the art, is employed using specific parameters in order to form extruded magnesium parts with properties that enable plastic deformation to be accomplished thereon in industrial applications, such as in the automotive industry. Fig. 1 illustrates an extrusion press 10 comprising a container 12 adapted to receive a magnesium billet 14, a ram 16, a die 18, and a floating mandrel (not seen in Fig. 1). The die 18 comprises an aperture 19 of a predetermined shape. The magnesium billet 14 is heated so that its temperature is within a range of 300°C to 605°C. The heated billet 14 is positioned in the container 12, and the die 18 is moved toward the billet 14, exerting a pressure which forces the billet 14 to deform, becoming an extrusion 20 which has a circumference similar to the aperture 19. The extrusion press 10 is adapted to maintain the billet 14 at the predetermined temperature during extrusion. The die 18 is moved at an extrusion rate substantially between 5 mm/sec and 45 mm/sec. The mandrel is positioned so that it forms a hollow 21 in the extrusion 20 and determines the size and shape of the hollow. The space between the die 18 and the mandrel determines the cross-sectional area of the extrusion 20. The extrusion reduction ratio is substantially between 10:1 and 50:1. When heating the magnesium billet 14, it should be kept in mind that additional heating will occur due to the pressure inherent to the extrusion process. Therefore, the billet 14 should not initially be heated to the desired temperature, so that it is not exceeded during the extrusion. The billet 14 used for the extrusion may be an undrilled billet, or a predrilled billet having a hollow center. The magnesium used in this process may be any commercially available magnesium alloy, such as AM60, AS41, AZ31, AZ61, AZ80, AZ91, ZE41, or ZM21. Alternatively, it may be a custom-made alloy. Preferably, the magnesium used with the process of the present invention is either the AZ31 or ZM21 alloy. The combination of parameters for any given magnesium alloy may be determined by one skilled in the art by trial and error. According to one particular embodiment, the chemical composition of the magnesium alloy used in the process according to the present invention is 2.856% Al, 1.022% Zn, 0.329% Mn, 0.004% Fe, 0.038% Si, 0.001% Cu, and 0.001%) Ni. In one experiment performed, a continuous casting system was used with a flat die of 42 mm, a mandrel of 38 mm and a container of 110 mm. The magnesium billet was 155 mm in length, 107 mm in diameter and was predrilled with a hole diameter of 38 mm (need to confirm pre-drilled). The extrusion rate was 1.6 mm/sec, with a billet and container heated to 320°C. The extrusion reduction ratio was about 30:1 with an overall force of 4.45 MN. The magnesium tube obtained using the above-described process had mechanical properties which provide the strength and durability to withstand, without failure, plastic deformations inherent in further production involving the tube. Specifically, it had a yield strength of 195 N/mm , an ultimate tensile strength (UTS) of 255 N/mm , and a 14% elongation at fracture. One process for which the magnesium tube obtained as described above may be used is internal high pressure forming. With reference to Fig. 2, this is accomplished with the aid of a specialized tooling 22. The tooling 22 comprises a clamping unit 25 disposed on each side of the tube 23 and a forming unit 27 surrounding it. The clamping unit 25 comprises crossheads 24, hydraulic cylinders 26, sealing punches 28, and appropriate heating and cooling means. The sealing punches 28 are adapted to seal the ends of the tube during forming, and at least one comprises an opening 42 adapted to introduce a pressure medium from a pressure source (not shown) into the tube. The forming unit 27 comprises body material 30, dies 32 which form an expansion zone 36, inserts 34 which form guiding zones 38, and appropriate heating and cooling means. Referring to Fig. 3, the tube 23 is deformed within the tooling 22. When the tube 23 is retained in the tooling, its ends are sealed, and a pressure medium is introduced at a forming pressure therein through the opening 42. A high pressure is applied to the medium, and an axial compression force (indicated by arrows 44) is applied to the tube 23. The expansion zone 36 is maintained at a temperature, substantially in the range of 200°C to 605°C, to permit the necessary circumferential strain for forming. In the guiding zone 38 a lower temperature is maintained, for example, in the range of 100°C to 200°C. This is to ensure that the flow stress of the portion of the tube 23 in the guiding zone 38 is sufficient to transfer the axial force to the portion of the tune in the expansion zone 36. (For example, depending on the alloy used, in the temperature range of about 350°C to 400°C, the flow stress can decrease to 40 N/mm2. The higher the axial force that is transferred to the portion of the tube in the expansion zone, the higher the circumferential strain that can be achieved, which leads to higher formability.) As a result, the tube 23 deforms in the expansion zone 36, and forms a bulge 40 which takes the shape of the die 32. It will be appreciated to one skilled in the art that the forming pressure is determined based on the magnesium alloy used to manufacture the tube, the thickness thereof, the specific geometry of the part to be fonned, and the temperature used for forming. A smaller radius and a lower temperature require a higher forming pressure. In addition, a thicker wall requires a higher forming pressure. The pressure medium is a fluid, being either a gas or a heat resistant fluid.
According to one embodiment, it is a gas which does not react with any other material it will come in contact with during the course of IHPF. It is preferably recoverable for subsequent use. Specifically, nitrogen or one of the noble gasses is used. Using a gas has several advantages over using a liquid, in that gasses may be heated to high temperatures as described with respect to the processes herein without undergoing decomposition. The formability of the magnesium tube during IHPF is partially influenced by the strain rate of the material. This influence increases with higher temperatures. Depending on process time and necessary formability, the strain rate may vary between 2χ 10_1sec-1 and 1 x 10_4sec_1. Previous heat treatment may also influence the initial structure of the magnesium tube. The tubes may be annealed at temperatures that are substantially between 200°C and 600°C. In one preferred case, the annealing temperature is between 250°C and 300°C. When annealed in this temperature range for a maximum of 6 hours, a uniform, fine-grained structure may be observed in the tube. A grain size between lOμm and 50μm can be realized. This fine-grained structure leads to an improved formability, especially at low strain rates (smaller then 2χl 0_1sec_1). The process described herein, and more specifically, the steps which involve IHPF may additionally be followed by subsequent IHPF operations in order to further deform or provide additional structural modifications to the tube. According to one example, the following conditions are used for IHPF. Subsequent to extrusion, the magnesium tube is annealed at 300°C for 6 hours. This annealing time leads to a uniform, fine-grained structure. One who is versed in the art will appreciate that a fine grain structure is particularly suitable for IHPF and similar processes. Thereafter, the magnesium tubes are preheated to a forming temperature of 350°C. The expansion zone is kept at a temperature of 350°C, and the guided zone is kept at a temperature of 250°C. At 350°C, the total elongation allowed is near a peak of about 35%. An axial force is applied by the hydraulic cylinders, which causes a compressive stress condition in the wall of the tube. As the pressure medium, nitrogen gas is used. The pressure vs. time path ensures a constant strain rate over the process time.

Claims

CLAIMS:
I. An article made of a magnesium alloy tube, the article having a grain size of between lOμm and 50μm and being manufactured by internal high pressure forming.
2. An article according to Claim 1, wherein the temperature of the internal high pressure forming is between 200°C and 605 °C.
3. An article according to Claim 1, wherein the tube was manufactured by extrusion.
4. An article according to Claim 3, wherein the extrusion temperature is between 300°C and 605°C.
5. An article according to Claim 3, wherein the extrusion speed is substantially between 5 mm/sec and 45 mm/sec.
6. An article according to Claim 3, wherein the extrusion reduction ratio is substantially between 10:1 and 50:1.
7. An article according to Claim 3, wherein the extrusion temperature is between 300°C and 605°C, the extrusion speed is substantially between 5 mm sec and 45 mm/sec, and the extrusion reduction ratio is substantially between 10:1 and 50:1.
8. An article according to any one of the above claims, wherein the magnesium alloy is selected from the group consisting of AZ31 and ZM21.
9. An article according to Claim 8, wherein the extrusion reduction ratio is substantially 30:1, the extrusion speed is substantially 15 mm/sec, the predetermined temperature is substantially 300°C, and the AZ31 alloy is used.
10. An article according to Claim 1, wherein the magnesium alloy comprises 2.856% aluminum, 1.022% zinc, 0.329% manganese, 0.004% iron, 0.038% silicon, 0.001 % copper, and 0.001 % nickel.
II. An article according to Claim 1, wherein the tube is annealed.
12. An article according to Claim 11, wherein the tube is annealed at a temperature of 300°C for six hours.
13. A process for manufacture of a tube from a billet made of a magnesium alloy, the process comprising: (a) heating the billet to a predetermined temperature that is within a range of 300°C to 605°; (b) extruding the billet, using an extrusion press having a ram, an internal piercing mandrel, and a die, while maintaining the temperature of the billet to stay within the range; and (c) applying a force to the billet so that it is forced between the die and the mandrel at a predetermined extrusion speed of the ram to form a tube having a predetermined extrusion reduction ratio; wherein the extrusion speed is substantially between 5 mm/sec and 45 mm/sec, and the extrusion reduction ratio is substantially between 10:1 and 50:1.
14. A process according to Claim 13, wherein the magnesium alloy is selected from the group consisting of AZ31 and ZM21.
15. A process according to Claim 14, wherein the extrusion reduction ratio is substantially 30:1, the extrusion speed is substantially 15 mm/sec, the predetermined temperature is substantially 300°C, and the AZ31 alloy is used.
16. A process according to Claim 1, wherein the magnesium alloy comprises 2.856% aluminum, 1.022% zinc, 0.329% manganese, 0.004% iron, 0.038% silicon, 0.001% copper, and 0.001% nickel.
17. A process according to Claim 1, wherein the process further comprises the step of annealing the tube.
18. A process according to Claim 17, wherein the tube is annealed at a temperature of 300°C for six hours.
19. A process according to Claim 13, further comprising the steps of (d) cooling the tube at a predetermined first cooling temperature for a predetermined amount of time; (e) sealing the tube from both ends; (f) introducing a pressure medium into the tube; (g) positioning the tube in a mold having a guiding zone at a predetermined guiding temperature and an expansion zone of a predetermined shape at a predetermined expansion temperature; (h) applying an axial compression force on the tube so that a section of the tube located in the expansion zone expands to conform to the predetermined shape; and (i) cooling the tube at a predetermined second cooling temperature for a predetermined amount of time; wherein the expansion temperature is within a range of 200°C to 605°.
20. A process according to Claim 19, wherein the expansion temperature is substantially between 200°C and 500°C.
21. A process according to Claim 19, wherein the pressure medium is a gas.
22. A process according to Claim 21, wherein the gas does not react with the metal under the conditions used in the process.
23. A process according to claim 19, wherein the pressure medium is a heat resistant liquid.
PCT/IL2005/000246 2004-03-02 2005-03-02 An article made of a magnesium alloy tube WO2005084845A1 (en)