KR101285690B1 - Manufacturing method of impedance matching and one electromagnetic shielding type relationship limit film - Google Patents

Manufacturing method of impedance matching and one electromagnetic shielding type relationship limit film Download PDF

Info

Publication number
KR101285690B1
KR101285690B1 KR1020130013147A KR20130013147A KR101285690B1 KR 101285690 B1 KR101285690 B1 KR 101285690B1 KR 1020130013147 A KR1020130013147 A KR 1020130013147A KR 20130013147 A KR20130013147 A KR 20130013147A KR 101285690 B1 KR101285690 B1 KR 101285690B1
Authority
KR
South Korea
Prior art keywords
insulating film
impedance matching
shielding
adhesive
electromagnetic shielding
Prior art date
Application number
KR1020130013147A
Other languages
Korean (ko)
Inventor
함원상
김헌균
장다원
이인섭
심희준
Original Assignee
신창핫멜트 주식회사
주식회사 영 신
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 신창핫멜트 주식회사, 주식회사 영 신 filed Critical 신창핫멜트 주식회사
Priority to KR1020130013147A priority Critical patent/KR101285690B1/en
Application granted granted Critical
Publication of KR101285690B1 publication Critical patent/KR101285690B1/en

Abstract

PURPOSE: A method of manufacturing an insulating film with an integrated impedance matching and electromagnetic shielding function is provided to reduce power consumption by using low voltage. CONSTITUTION: An insulating film is manufactured by spreading an insulating adhesive (S110). A film for impedance matching and electromagnetic shielding is manufactured (S120). The adhesive is stabilized in a curing room (S130). An insulating film with an integrated impedance matching and electromagnetic shielding function is manufactured (S140). The integrated adhesive is secondarily stabilized (S150). [Reference numerals] (S110) Step of manufacturing an insulating film; (S111) Step of drawing the insulating film; (S112) Step of spreading an insulating adhesive; (S120) Step of a film for impedance matching and electromagnetic shielding; (S121) Step of drawing the insulating film for impedance matching and shielding; (S122) Step of spreading an adhesive; (S123) Step of attaching aluminum; (S130) Step of stabilization; (S140) Step of manufacturing an insulating film with an integrated impedance matching and electromagnetic function; (S150) Step of secondary stabilization

Description

임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법{manufacturing method of impedance matching and one electromagnetic shielding type relationship limit film }Manufacturing method of impedance matching and one electromagnetic shielding type relationship limit film}

본 발명은 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법에 관한 것으로서, 보다 상세하게는 일련된 공정을 통하여 임피던스매칭 및 전자파 차폐가 가능한 절연필름을 제조가능하게 구성함으로써, 제조 공정의 축소로 인한 제조단가를 낮출 수 있도록 한 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법에 관한 것이다.
The present invention relates to a method for manufacturing an impedance matching and electromagnetic shielding integral insulating film, and more particularly, to manufacture an insulating film capable of impedance matching and electromagnetic shielding through a series of processes, thereby manufacturing by reducing the manufacturing process. The present invention relates to a method of manufacturing an impedance matching and electromagnetic shielding-integrated insulating film to lower the unit cost.

주지하는 바와 같이 디지털 가전 제품에 있어서 모든 데이터는 전기적 신호로 전송되며, 특히, 고성능의 디지털 가전 제품의 경우에는 각종 부품들 간 또는 각종 기기 간에 대량의 데이터를 정보 손실없이 효과적으로 전송할 수 있는 시스템이 요구된다. As is well known, all data is transmitted as an electrical signal in a digital home appliance. In particular, a high-performance digital home appliance requires a system capable of effectively transferring a large amount of data between various parts or between various devices without loss of information. do.

이와 같이, 디지털 가전 제품에서는 신호 전달 성능이 그 제품의 성능으로 직결되기 때문에 데이터전송 시스템에 대한 성능 향상의 노력이 중점적으로 이루어지고 있으며, 이러한 디지털 가전 제품의 성능 향상을 위하여, 데이터 전송량의 증가에 따른 신호 전송 속도의 고속화를 구현할 수 있도록 사용 주파수의 고주파와 함께 새로운 인터페이스 기술이 요구되고 있다.As such, since signal transmission performance is directly related to the performance of the product, efforts to improve the performance of the data transmission system have been focused on the digital home appliances, and in order to improve the performance of the digital home appliances, A new interface technology is required along with the high frequency of the use frequency to realize the high speed of the signal transmission.

이와 관련하여, 낮은 전압을 사용함으로써 전력소모를 감소시킬 수 있으며, 고속 전송이 가능하며 전송거리가 긴 저전압 차분 신호(Low Voltage Differential Signaling: 이하, 'LVDS' 라고 한다.) 솔루션이 폭넓게 사용되고 있다.In this context, the use of low voltages can reduce power consumption, enable high-speed transmission, and have long transmission distances. Low Voltage Differential Signaling (LVDS) solutions are widely used.

상기한 저전압 차분 신호(LVDS)란 고속 데이터 전송을 위한 일반적인 인터페이스 표준을 의미하는 것으로서, 디지털 기기의 데이터 전송시스템을 포함한 다양한 분야에 적용되고 있는 기술이다.The low voltage differential signal (LVDS) refers to a general interface standard for high speed data transmission, and is applied to various fields including a data transmission system of a digital device.

특히, 디지털 기기의 시스템 내부적으로 대용량의 데이터를 고속 전송하기 위하여 이러한 저전압 차분 신호 솔루션이 주로 사용되고 있으며, 디스플레이 장치와 같은 디지털 기기에서는 데이터 전송을 위한 전송 매체로는 연성인쇄기판(Flexible Print Circuit ; FPC)과 동등한 연성과 전송 특성을 가지면서 제조 비용이 낮은 연성 평판 케이블(Flexible Flat Cable: FFC)이 많이 사용되어 저전압 차분 신호 솔루션이 구현된다.In particular, such a low voltage differential signal solution is mainly used for high-speed transmission of a large amount of data in a system of a digital device, and in a digital device such as a display device, a flexible print circuit (FPC) is used as a transmission medium for data transmission. Flexible Flat Cables (FFCs), which are equal in ductility and transmission characteristics, and have low manufacturing costs, are used to achieve low-voltage differential signaling solutions.

종래의 일반적인 EMI 저감형 LVDS용 연성 평판 케이블은, 내부에 자성 분말이 도포된 복합 자성체 층을 포함하고, 도체 및 상기 도체의 상·하부에 협착된 상부 및 하부 절연체와 접지단자에 연결된 금속 실드재를 포함하도록 구성할 수 있으며, 상기 금속 실드재 내측으로 자성분말이 도포된 복합 자성체 층이 형성되도록 구성된다.Conventional flat EMI cables for EMI-reducing LVDS include a composite magnetic layer coated with magnetic powder therein, and a metal shield material connected to the conductor and the upper and lower insulators clamped on the upper and lower portions of the conductor and the ground terminal. It can be configured to include, and is configured to form a composite magnetic material layer is applied to the magnetic powder inside the metal shielding material.

그러나, 상기한 종래의 일반적인 저전압 차분 신호용 연성 평판 케이블은, 신호 전송시 전자파를 흡수하지 못하고 반사하게 되므로 인해 삽입로스(Insertion Loss)와, 누화(Cross Talk) 그리고 반사 손실(Return Loss)의 열화로 인한 신호 전달이 제대로 되지 않아 3Gbps가 넘는 고속성에서는 사용할 수 없는 문제점이 있었다.However, the above-described conventional flat cable for low voltage differential signal, because it is reflected by the electromagnetic wave does not absorb the signal transmission, due to degradation of insertion loss, cross talk, and return loss. Due to poor signal transmission, there was a problem that can not be used at high speeds over 3Gbps.

이러한 점을 감안하여 특허출원번호 10-2011-0015674호로 저전압 차분신호용 연성 평판 케이블이 출원된바 있다.In view of this point, the patent application No. 10-2011-0015674 has been filed a flexible flat cable for low voltage differential signal.

살펴보면, 종래의 일반적인 저전압 차분신호용 연성 평판 케이블은, 저전압 차분신호용 연성 평판 케이블에 있어서, 상부 및 하부 절연필름과, 상기 상부 및 하부 절연필름 사이에 양단 일면이 외부로 노출되게 서로 일정한 간격으로 1개 이상의 그라운드선 및 신호선을 포함하여 다수개 배열시켜 열융착장치를 통하여 열융착되어 고정되는 도체와, 상기 상부 절연필름 또는 하부절연필름 또는 상부 및 하부절연필름의 양면에 유전체접착용접착부재를 매개로 점착되어 신호 전달시 저손실 특성임피던스를 이루도록 공극형 실리카 또는 탄산칼슘이나 유기폴리머로 코팅된 공극형 실리카 유기폴리머를 포함하여 구비되는 유전체층과, 상기 유전체층 상면에 도포되어 신호 전달시 발생되는 전자파를 흡수가능하도록 구비되는 전자파흡수층과, 상기 전차파흡수층의 상면에 열융착되어 절연가능하도록 구비되는 절연부재와, 상기 절연부재의 상면에 구비되는 절연부재 접착용접착부재를 매개로 접착되어 구비되는 금속도전부재를 포함하여 이루어진다.Looking at the conventional low-voltage differential signal flexible flat cable, a low-voltage differential signal flexible flat cable, the upper and lower insulating film and the upper and lower insulating film between the upper and lower insulating film one at a regular interval from each other to be exposed to the outside. A plurality of conductors including ground lines and signal lines are arranged to be heat-sealed and fixed through a heat welding apparatus, and a dielectric adhesive bonding member is formed on both sides of the upper insulating film or the lower insulating film or the upper and lower insulating films. A dielectric layer comprising pore type silica or a pore type silica organic polymer coated with calcium carbonate or an organic polymer so as to achieve low loss characteristic impedance during signal transmission, and absorbing electromagnetic waves generated when the signal is applied to the dielectric layer. An electromagnetic wave absorbing layer and the electric wave It includes an insulating member provided to be insulated and heat-sealed on the upper surface of the absorbing layer, and a metal conductive member attached to the insulating member adhesive bonding member provided on the upper surface of the insulating member.

그러나 이와 같이 이루어진 종래의 일반적인 저전압 차분신호용 연성 평판 케이블은 상기한 바와 같이 저전압 차분신호용 연성 평판 케이블을 제조한 후, 제조된 저전압 차분신호용 연성 평판 케이블의 일면 또는 양면 즉, 상부 절연필름 또는 하부 절연필름 또는 상부 및 하부 절연필름에 전자파 흡수층을 부착하는 것에 의해 제조되는바, 저전압 차분신호용 연성 평판 케이블의 제조를 위한 공정이 복잡하므로 인해 제조 단가가 상승될 수 밖에 없는 문제점이 있었다.
However, in the conventional general low voltage differential signal flexible flat cable made as described above, after manufacturing the low voltage differential signal flexible flat cable as described above, one or both sides of the manufactured low voltage differential signal flexible flat cable, that is, the upper insulating film or the lower insulating film Alternatively, the bar is manufactured by attaching an electromagnetic wave absorbing layer to the upper and lower insulating films, and thus, a manufacturing cost increases due to a complicated process for manufacturing a flexible flat cable for low voltage differential signal.

특허출원번호 10-2011-0015674호, 출원일; 2011년02월22일Patent Application No. 10-2011-0015674, filed date; February 22, 2011 발명의 명칭: 저전압 차분신호용 연성 평판 케이블, 도 1Title of the Invention: Flexible flat cable for low voltage differential signal, FIG.

이에, 본 발명은 상술한 문제점을 해소하기 위해 안출된 것으로서, 일련된 공정을 통하여 임피던스매칭 및 전자파 차폐가 가능한 절연필름을 제조가능하게 구성함으로써, 제조 공정의 축소로 인한 제조단가를 낮출 수 있도록 한 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법을 제공함에 그 목적이 있다.Accordingly, the present invention has been made in order to solve the above problems, by making an insulating film capable of impedance matching and electromagnetic shielding through a series of processes, it is possible to lower the manufacturing cost due to the reduction of the manufacturing process An object of the present invention is to provide a method of manufacturing an impedance matching and electromagnetic shielding integrated insulating film.

본 발명의 다른 목적들은 기술이 진행되면서 명확해질 것이다.
Other objects of the present invention will become apparent as the description proceeds.

상술한 목적을 달성하기 위한 본 발명은, 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법에 있어서, 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조장치의 제어부에 의해 구동하는 인출용구동모터의 구동으로 권취롤에 권취된 절연용필름이 인출되는 중에 일면에 절연용접착제가 도포되는 것에 의해 절연용필름을 제조하는 단계와, 상기 단계에 의해 제조된 절연용필름의 타면에 부착되는 것에 의해 임피던스매칭 및 전자파를 차폐가능하도록 차폐용절연필름권취롤과 알루미늄권취롤에 각각 권취된 차폐용절연필름과 박판의 알루미늄이 각각의 구동모터 구동으로 각각 인출되는 중에 접착제를 매개로 접착되어 임피던스매칭 및 전자파 차폐용필름을 제조하는 단계와, 상기 단계에 의해 제조된 임피던스매칭 및 전자파 차폐용필름에 포함된 접착제를 숙성실에서 안정화시키는 단계와, 상기 단계에 의해 안정화된 임피던스매칭 및 전자파 차폐용 필름과 상기 단계에 의해 제조된 절연용필름 사이에 일체용접착제를 개재시켜 가압로울러를 통과하는 것에 의해 임피던스매칭 및 전자파 차폐 일체형 절연필름을 제조하는 단계를 포함하여 이루어진 것을 특징으로 한다.The present invention for achieving the above object, in the method of manufacturing an impedance matching and electromagnetic shielding integral insulating film, wound by the drive of the drive motor for drawing drive driven by the control unit of the manufacturing apparatus of the impedance matching and electromagnetic shielding integral insulating film. While the insulating film wound on the roll is taken out, an insulating adhesive is applied to one surface to prepare the insulating film, and by attaching to the other surface of the insulating film manufactured by the above step, impedance matching and electromagnetic wave The shielding insulating film wound on the shielding film winding roll and the aluminum winding roll and the aluminum of the thin plate respectively are pulled out by the respective driving motor driving so as to shield the film. To prepare a, and to the film for impedance matching and electromagnetic shielding prepared by the step Stabilizing the included adhesive in the aging chamber, and the impedance by passing through the pressure roller by interposing an integral adhesive between the film for the impedance matching and electromagnetic shielding stabilized by the step and the insulating film prepared by the step It characterized in that it comprises a step of manufacturing a matching and electromagnetic shielding integral insulating film.

또한, 상기한 단계에 의해 임피던스매칭 및 전자파 차폐 일체형 절연필름으로 제조된 후에는 접착제의 안정화를 위해 50℃~70℃의 내부온도를 갖는 숙성실에서 24시간~48시간 동안 체류시켜 접착제를 2차 안정화시키는 단계를 더 포함하여 이루어진 것을 특징으로 한다.In addition, after the impedance matching and electromagnetic shielding-integrated insulating film by the above step, to stabilize the adhesive in the aging room having an internal temperature of 50 ℃ ~ 70 ℃ 24 hours to 48 hours to stabilize the adhesive secondary Characterized in that further comprises the step of.

삭제delete

상기한 바와 같이 본 발명에 따른 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법에 따르면, 일련된 공정을 통하여 임피던스매칭 및 전자파 차폐가 가능한 절연필름을 제조가능하게 구성함으로써, 제조 공정의 축소로 인한 제조단가를 낮출 수 있고, 일련의 공정에 의해 임피던스매칭 및 전자파 차폐 일체형 절연필름를 제조하게 되므로 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조시 불량률 감소시킬 수 있는 효과가 있다.
According to the manufacturing method of the impedance matching and electromagnetic shielding integral insulating film according to the present invention as described above, by making a manufacturing process capable of manufacturing an insulating film capable of impedance matching and electromagnetic shielding through a series of processes, manufacturing by reducing the manufacturing process Since the unit cost can be lowered and the impedance matching and electromagnetic shielding integral insulating film is manufactured by a series of processes, the defective rate can be reduced during the production of the impedance matching and electromagnetic shielding integral insulating film.

도 1은 본 발명에 따른 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법을 설명하기 위한 흐름도이다.
도 2는 본 발명에 따른 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법에 의해 제조된 임피던스매칭 및 전자파 차폐 일체형 절연필름을 도시한 도면이다.
1 is a flowchart illustrating a method of manufacturing an impedance matching and electromagnetic shielding integrated insulating film according to the present invention.
2 is a view showing an impedance matching and electromagnetic shielding integral insulating film manufactured by the method of manufacturing an impedance matching and electromagnetic shielding integral insulating film according to the present invention.

이하에서는, 본 발명에 따른 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법의 일실시예를 들어 상세하게 설명한다.Hereinafter, an embodiment of the manufacturing method of the impedance matching and electromagnetic shielding integral insulating film according to the present invention will be described in detail.

우선, 도면들 중, 동일한 구성요소 또는 부품들은 가능한 한 동일한 참조부호를 나타내고 있음에 유의하여야 한다. 본 발명을 설명함에 있어, 관련된 공지기능 혹은 구성에 대한 구체적인 설명은 발명의 요지를 모호하지 않게 하기 위하여 생략한다. First, it should be noted that, in the drawings, the same components or parts have the same reference numerals as much as possible. In describing the present invention, a detailed description of known functions and configurations incorporated herein will be omitted so as not to obscure the gist of the invention.

도면을 설명하기에 앞서, 본 발명의 기본적인 개념은 임피던스매칭 및 전자파 차폐 그리고 절연이 가능한 필름을 일련의 공정을 통하여 한 번에 제조가능하도록 함으로써, 임피던스매칭 및 전자파 차폐 그리고 절연이 가능한 필름의 제조에 따른 공정 축소로 제조비용을 절감시킬 수 있도록 한 것에 있음을 밝혀 둔다.Prior to describing the drawings, the basic concept of the present invention is to produce a film capable of impedance matching, electromagnetic shielding and insulation by making a film capable of impedance matching and electromagnetic shielding and insulation at one time through a series of processes. It is to be noted that it is possible to reduce the manufacturing cost by reducing the process.

다음, 첨부된 도면을 참조하면서 위와 같은 기본적인 개념을 갖는 본 발명에 따른 임피던스매칭 및 전자파 차폐 일체형 절연필름 제조방법의 바람직한 실시양태를 설명한다.Next, with reference to the accompanying drawings will be described a preferred embodiment of the impedance matching and electromagnetic shielding integrated insulating film manufacturing method according to the present invention having the above basic concept.

첨부된 도면 도 1은 본 발명에 따른 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법을 설명하기 위한 흐름도이다.1 is a flowchart illustrating a method of manufacturing an impedance matching and electromagnetic shielding integrated insulating film according to the present invention.

도시된 바와 같이 본 발명에 따른 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법은, 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조장치의 제어부에 의해 구동하는 인출용구동모터의 구동으로 권취롤에 권취된 절연용필름이 인출되는 중에 일면에 절연용접착제가 도포되는 것에 의해 절연용필름을 제조하는 단계(S110)와, 상기 단계(S110)에 의해 제조된 절연용필름의 타면에 부착되는 것에 의해 임피던스매칭 및 전자파를 차폐가능하도록 차폐용절연필름권취롤과 알루미늄권취롤에 각각 권취된 차폐용절연필름과 박판의 알루미늄이 각각의 구동모터 구동으로 각각 인출되는 중에 접착제를 매개로 접착되어 임피던스매칭 및 전자파 차폐용필름을 제조하는 단계(S120)와, 상기 단계(S120)에 의해 제조된 임피던스매칭 및 전자파 차폐용필름에 포함된 접착제를 숙성실에서 안정화시키는 단계(S130)와, 상기 단계(S130)에 의해 안정화된 임피던스매칭 및 전자파 차폐용 필름과 상기 단계에 의해 제조된 절연용필름 사이에 일체용접착제를 개재시켜 가압로울러를 통과하는 것에 의해 임피던스매칭 및 전자파 차폐 일체형 절연필름을 제조하는 단계(S140)를 포함하여 이루어진다.As shown, the method of manufacturing the impedance matching and electromagnetic shielding integral insulating film according to the present invention is wound on the take-up roll by the driving of the take-out driving motor driven by the controller of the apparatus for manufacturing the impedance matching and electromagnetic shielding integral insulating film. While the insulating film is drawn out, an insulating adhesive is applied to one surface to prepare an insulating film (S110) and impedance matching by being attached to the other surface of the insulating film manufactured by the step (S110). And the shielding insulating film wound on the shielding film winding roll and the aluminum winding roll and the aluminum of the thin plate respectively being drawn out by the respective driving motor driving to shield the electromagnetic waves. A step of preparing a film for operation (S120), and the impedance matching and electromagnetic shielding peeling prepared by the step (S120) Stabilizing the adhesive contained in the aging room (S130), and the pressure between the impedance matching and electromagnetic shielding film stabilized by the step (S130) and the insulating film prepared by the step interposed through the integral adhesive Passing through the roller is made, including the step of manufacturing an impedance matching and electromagnetic shielding integral insulating film (S140).

또한, 상기한 단계(S140)에 의해 임피던스매칭 및 전자파 차폐 일체형 절연필름으로 제조된 후에는 접착제의 안정화를 위해 50℃~70℃의 내부온도를 갖는 숙성실에서 24시간~48시간 동안 체류시켜 일체용접착제를 2차안정화시키는 단계(S150) 후 제품을 출하하도록 구성된다. In addition, after the impedance matching and electromagnetic shielding integral insulating film is prepared by the above step (S140) to maintain the adhesive for stabilizing the adhesive for 24 hours to 48 hours in a aging room having an internal temperature of 50 ℃ ~ 70 ℃ After stabilizing the adhesive (S150) it is configured to ship the product.

한편, 상기한 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법에 의해 제조된 임피던스매칭 및 전자파 차폐 일체형 절연필름(200)은, 첨부된 도면 도 2에 도시된 바와 같이 일면에 이형지(210)가 부착되어 절열가능하게 구비되는 절연필름층(220)과, 상기 절연필름층(220)의 타면에 일체용접착제(230)를 매개로 부착되는 것에 의해 임피던스매칭 및 전자파를 차폐가능하도록 구비되는 임피던스매칭 및 전자파 차폐층(240)을 포함하여 이루어진다.On the other hand, the impedance matching and electromagnetic shielding integral insulating film 200 manufactured by the method of manufacturing the impedance matching and electromagnetic shielding integral insulating film 200, the release paper 210 is attached to one surface as shown in FIG. Impedance matching and impedance matching and electromagnetic wave shielding are provided by attaching the insulating film layer 220 and the other surface of the insulating film layer 220 to the other surface of the insulating film layer 220 through the integral adhesive agent 230, It comprises an electromagnetic shielding layer 240.

여기서, 상기한 절연필름층(220)은 절연필름(221)과, 상기 절연필름(221)의 일면에 이형지(210)를 부착시킬 수 있도록 구비되는 절연용접착제(221)로 구성된다. Here, the insulating film layer 220 is composed of an insulating film 221 and the insulating adhesive 221 provided to attach the release paper 210 to one surface of the insulating film 221.

또한, 상기한 임피던스매칭 및 전자파 차폐층(240)은 상기 절연필름층(220)의 타면에 일체용접착제(230)를 매개로 부착가능하게 구비되는 임피던스매칭 및 차폐용 절연필름층(241)과, 상기 임피던스매칭 및 차폐용 절연필름층(241)의 타면에 접착제(242)를 매개로 부착되어 전자파를 차폐가능하도록 구비되는 박막의 알루미늄층(243)으로 구성된다. In addition, the impedance matching and electromagnetic shielding layer 240 and the impedance matching and shielding insulating film layer 241 which is provided to be attached to the other surface of the insulating film layer 220 through the integral adhesive 230. The thin film aluminum layer 243 is attached to the other surface of the impedance matching and shielding insulating film layer 241 through an adhesive 242 to shield electromagnetic waves.

이하에서, 상기한 본 발명에 따른 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법에 대하여 보다 상세하게 설명하면 다음과 같다.Hereinafter, a method of manufacturing the impedance matching and electromagnetic shielding integral insulating film according to the present invention will be described in more detail.

먼저, 본 발명에 따른 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법의 절연용필름을 제조하는 단계(S110)는, 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조장치의 제어부에 의해 인출용구동모터가 구동하는 것에 대응되게 권취롤에 권취된 절연용필름이 인출되는 단계(S111)와, 상기 단계(S111)에 의해 절연용필름이 권취롤로부터 인출되면서 이송되면, 제어부의 제어에 의해 개폐밸브가 개방되는 것에 대응되게 절연용접착제저장부로부터 공급되는 절연용접착제가 절연용필름의 일면에 도포되는 단계(S112)로 구성된다.First, the step (S110) of manufacturing the insulation film of the method of manufacturing the impedance matching and electromagnetic shielding integral insulating film according to the present invention, the driving motor for drawing out by the control unit of the manufacturing apparatus of the impedance matching and electromagnetic shielding integral insulating film When the insulating film wound on the take-up roll is taken out to correspond to driving (S111) and the insulating film is taken out from the take-up roll by the step (S111), the opening / closing valve is opened by the control of the controller. Corresponding to being made is the step of applying the insulating adhesive supplied from the insulating adhesive storage unit on one surface of the insulating film (S112).

상기한 임피던스매칭 및 전자파 차폐용 필름 제조단계(S120)는, 상기 단계(S110)에 의해 제조된 절연용필름의 타면에 부착되어 임피던스매칭 및 전자파 차폐를 위한 임피던스매칭 및 전자파 차폐용 필름을 제조하는 단계이다. The impedance matching and electromagnetic wave shielding film manufacturing step (S120) is attached to the other surface of the insulating film prepared by the step (S110) to produce an impedance matching and electromagnetic shielding film for impedance matching and electromagnetic shielding Step.

즉, 상기한 임피던스매칭 및 전자파 차폐용 필름 제조단계(S120)는 차폐용절연필름권취롤에 권취되어 구동모터가 제어부에 의해 구동하는 것에 의해 임피던스매칭 및 차폐용 절연필름이 인출되는 단계(S121)와, 상기 단계(S121)에 의해 임피던스매칭 및 차폐용 절연필름이 차폐용절연필름권취롤로부터 인출되면서 이송되면, 제어부의 제어에 의해 개폐밸브가 개방되는 것에 대응되게 접착제저장부로부터 공급되는 접착제가 임피던스매칭 및 차폐용 절연필름의 일면에 도포되는 단계(S122)와, 상기 단계(S122)에 의해 이송중인 임피던스매칭 및 차폐용 절연필름의 일면에 접착제가 도포되면, 알루미늄권취롤에 권취되어 알루미늄인출용구동모터가 제어부에 의해 구동하는 것에 의해 접착제 타면측으로 박판의 알루미늄이 인출되어 부착되는 단계(S123)로 구성된다.That is, the above-mentioned impedance matching and electromagnetic shielding film manufacturing step (S120) is wound on the insulating film winding roll for shielding and driving the driving motor by the control unit to pull out the impedance matching and shielding insulating film (S121). And, when the impedance matching and shielding insulating film is drawn out from the shielding insulating film winding roll by the step (S121) and transported, the adhesive supplied from the adhesive storage unit corresponding to the opening and closing valve is opened by the control of the control unit When the adhesive is applied to one surface of the impedance matching and shielding insulating film being transported by the step (S122) and the transfer of the impedance matching and shielding insulating film by the step (S122), it is wound on an aluminum winding roll to draw aluminum The driving motor is driven by the control unit is configured to take out the aluminum of the thin plate to the other side of the adhesive is attached to (S123) The.

상기한 안정화 단계(S130)는 임피던스매칭 및 전자를 차폐용필름 제조에 따른 접착제를 숙성실에서 장시간 안정시키는 단계이다.The stabilization step (S130) is a step of stabilizing the adhesive in the maturation room for a long time in accordance with the impedance matching and electron shielding film production.

즉, 상기 임피던스매칭 및 차폐용 절연필름이 차폐용절연필름권취롤로부터 인출되어 이동하는 중에 일면에 접착제가 도포되므로 접착제는 불안정한 상태로서 안정을 시키기 위한 단계이다.That is, since the adhesive is applied to one surface while the impedance matching and shielding insulating film is withdrawn from the shielding insulating film winding roll, the adhesive is a step for stabilizing as an unstable state.

이때, 상기한 숙성실의 온도는 접착제의 안정화를 위해 50℃~70℃의 온도범위를 유지하고, 상기 온도 범위에서 접착제가 안정화될 수 있도록 24시간~48시간 동안 숙성실에서 보관된다.
In this case, the temperature of the aging chamber is maintained in a temperature range of 50 ℃ to 70 ℃ for the stabilization of the adhesive, and stored in the aging room for 24 to 48 hours to stabilize the adhesive in the temperature range.

이와 같이 이루어진 본 발명에 따른 임피던스매칭 및 전자파 차폐 일체형 절연필름 제조방법을 통하여 임피던스매칭 및 전자파 차폐 일체형 절연필름을 제조하고자 할 경우에는 첨부된 도면 도 1 및 도 2에 도시된 바와 같이 먼저, 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조장치의 제어부에 갖추어진 작동버튼을 누름시키는 것에 의해 구동하는 인출용구동모터가 구동하게 된다.In order to manufacture the impedance matching and electromagnetic shielding integral insulating film through the impedance matching and electromagnetic shielding integrated insulating film manufacturing method according to the present invention made as described above, first, impedance matching as shown in Figs. And a drawing drive motor driven by pressing an operation button provided on a control unit of the manufacturing apparatus of the electromagnetic wave shield integrated insulating film.

상기 인출용구동모터의 구동으로 권취롤에 권취된 절연용필름(222)이 인출된다.The insulating film 222 wound on the take-up roll is drawn out by driving the take-out driving motor.

상기와 같이 절연용필름(222)이 인출되면, 제어부의 제어에 의해 절연용접착제저장부의 개폐밸브가 개방되는 것에 대응되게 절연용접착제(221)가 이동중인 절연용필름(222)의 일면에 도포되는 것에 의해 절연용필름의 제조가 완료된다.When the insulating film 222 is drawn as described above, the insulating adhesive 221 is applied to one surface of the insulating film 222 in which the insulating adhesive 221 is moving to correspond to the opening and closing valve of the insulating adhesive storage unit under control of the controller. The production of the insulating film is completed by the process.

상기와 같이 절연영필름의 제조가 완료되면, 제어부의 제어에 의해 구동모터가 구동하는 것에 대응되게 차폐용절연필름권취롤에 권취되어 있는 임피던스매칭 및 차폐용 절연필름(241)이 인출된다.When the preparation of the insulating film is completed as described above, the impedance matching and the shielding insulating film 241 wound on the shielding insulating film winding roll are drawn out corresponding to the driving of the driving motor under the control of the controller.

상기 임피던스매칭 및 차폐용 절연필름(241)이 인출되면 제어부의 제어에 의해 접착제저장부의 개폐밸브가 개방되는 것에 대응되게 접착제(242)가 이동중인 임피던스매칭 및 차폐용 절연필름(241)에 도포된다.When the impedance matching and shielding insulating film 241 is drawn out, the adhesive 242 is applied to the moving impedance matching and shielding insulating film 241 corresponding to the opening and closing valve of the adhesive storage unit under control of the controller. .

상기와 같이 임피던스매칭 및 차폐용 절연필름(241)의 일면에 접착제(242)가 도포되어 이송되면 제어부의 제어에 의해 알루미늄인출용구동모터가 구동하는 것에 대응되게 알루미늄권취롤에 권취되어 있는 박판의 알루미늄(243)이 인출되면서 접착제(242)에 부착되는 것에 의해 임피던스매칭 및 전자파 차폐용필름의 제조가 완료된다.As described above, when the adhesive 242 is applied and transferred to one surface of the impedance matching and shielding insulating film 241, the thin sheet is wound on the aluminum winding roll to correspond to the driving of the aluminum take-out driving motor under the control of the controller. The aluminum 243 is drawn out and attached to the adhesive 242 to complete the manufacture of the film for impedance matching and electromagnetic shielding.

상기와 같이 임피던스매칭 및 전자파 차폐용필름의 제조가 완료되면, 접착제를 안정화시키기 위해 60℃의 내부 온도를 갖는 숙성실에 48시간 동안 임피던스매칭 및 전자파 차폐용필름을 체류시킨다.When the preparation of the impedance matching and electromagnetic shielding film as described above is completed, the impedance matching and electromagnetic shielding film is left in the aging room having an internal temperature of 60 ° C. for 48 hours to stabilize the adhesive.

상기와 같이 숙성실에서 48시간 동안 체류되어 임피던스매칭 및 전자파 차폐용필름의 접착제가 안정화되면, 절연용필름(222)의 타면에 일체용접착제(230)를 개재시켜 가압로울러를 통과하는 것에 의해 임피던스매칭 및 전자파 차폐 일체형 절연필름(200)을 제조된다.If the adhesive of the film for impedance matching and electromagnetic wave shielding is stabilized in the aging room for 48 hours as described above, impedance matching by passing the pressure roller through the integral adhesive 230 on the other surface of the insulating film 222. And the electromagnetic wave shield integrated insulating film 200 is manufactured.

상기와 같이 제조된 임피던스매칭 및 전자파 차폐 일체형 절연필름(200)의 일체용접착제(230)를 안정화시키도록 60℃의 내부 온도를 갖는 숙성실에 48시간 동안 체류시켜 배출하는 것에 의해 임피던스매칭 및 전자파 차폐 일체형 절연필름(200)의 제조가 완료된다.Impedance matching and electromagnetic shielding by staying for 48 hours in a aging chamber having an internal temperature of 60 ° C. to stabilize the integral adhesive 230 of the impedance matching and electromagnetic shielding integrated insulating film 200 manufactured as described above. Manufacturing of the integral insulating film 200 is completed.

이상에서 설명한 본 발명은 전술한 실시예 및 첨부된 도면에 의해 한정되는것이 아니고, 본 발명의 기술적 사상을 벗어나지 않는 범위 내에서 여러 가지 치환, 변형 및 변경이 가능함은 본 발명이 속하는 기술 분야에서 통상의 지식을 가진 자에게 있어서 명백할 것이다.
It will be apparent to those skilled in the art that various modifications and variations can be made in the present invention without departing from the spirit or scope of the inventions. It will be clear to those who have knowledge of.

200 ; 임피던스매칭 및 전자파 차폐 일체형 절연필름
210 ; 이형지 220 ; 절연필름층
230 ; 일체용접착제 240 ; 임피던스매칭 및 전자파 차폐층
200; Impedance Matching and Electromagnetic Shielding Insulation Film
210; Release paper 220; Insulation film layer
230; Integral adhesive 240; Impedance matching and electromagnetic shielding layer

Claims (6)

임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법에 있어서,
임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조장치의 제어부에 의해 구동하는 인출용구동모터의 구동으로 권취롤에 권취된 절연용필름이 인출되는 중에 일면에 절연용접착제가 도포되는 것에 의해 절연필름을 제조하는 단계(S110)와;
상기 단계(S110)에 의해 제조된 절연필름의 타면에 부착되는 것에 의해 임피던스매칭 및 전자파를 차폐가능하도록 차폐용절연필름권취롤과 알루미늄권취롤에 각각 권취된 차폐용절연필름과 박판의 알루미늄이 각각의 구동모터 구동으로 각각 인출되는 중에 접착제를 매개로 접착되어 임피던스매칭 및 전자파 차폐용필름을 제조하는 단계(S120)와;
상기 단계(S120)에 의해 제조된 임피던스매칭 및 전자파 차폐용필름에 포함된 접착제를 숙성실에서 안정화시키는 단계(S130)와;
상기 단계(S130)에 의해 안정화된 임피던스매칭 및 전자파 차폐용 필름과 상기 단계에 의해 제조된 절연필름 사이에 일체용접착제를 개재시켜 가압로울러를 통과하는 것에 의해 임피던스매칭 및 전자파 차폐 일체형 절연필름을 제조하는 단계(S140)를
포함하여 이루어진 것을 특징으로 하는 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법.
In the manufacturing method of impedance matching and electromagnetic shielding integral insulating film,
An insulating film is manufactured by applying an insulating adhesive on one surface of the insulating film wound on the take-up roll while being driven by a drawing drive motor driven by a control unit of an impedance matching and electromagnetic wave shield integrated insulating film manufacturing apparatus. Step (S110);
The shielding insulating film and the aluminum of the thin film wound on the shielding insulating film winding roll and the aluminum winding roll, respectively, to be capable of shielding the impedance matching and electromagnetic waves by being attached to the other surface of the insulating film manufactured by the step (S110), respectively. A step of manufacturing a film for impedance matching and electromagnetic shielding by bonding the adhesive during the extraction of the driving motor of the drive (S120);
Stabilizing the adhesive included in the impedance matching and electromagnetic wave shielding film prepared by the step (S120) in a aging room (S130);
Impedance matching and electromagnetic shielding integral insulating film is produced by passing through a pressure roller with an integral adhesive between the film for impedance matching and electromagnetic shielding stabilized by the step (S130) and the insulating film prepared by the step. Step (S140)
Impedance matching and electromagnetic shielding integrated insulation film production method comprising a.
제1항에 있어서,
상기 단계(S140)에 의해 임피던스매칭 및 전자파 차폐 일체형 절연필름으로 제조된 후에는 접착제의 안정화를 위해 50℃~70℃의 내부온도를 갖는 숙성실에서 24시간~48시간 동안 체류시켜 접착제를 2차 안정화시키는 단계(S150)를 더 포함하여 이루어진 것을 특징으로 하는 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법.
The method of claim 1,
After manufacturing the impedance matching and electromagnetic shielding integral insulating film by the step (S140) to stabilize the adhesive in the aging room having an internal temperature of 50 ℃ ~ 70 ℃ 24 hours to 48 hours to stabilize the adhesive secondary Impedance matching and electromagnetic shielding integrated insulating film, characterized in that it further comprises the step (S150).
제1항에 있어서,
상기 임피던스매칭 및 전자파 차폐용 필름 제조단계(S120)는, 차폐용절연필름권취롤에 권취되어 구동모터가 제어부에 의해 구동하는 것에 의해 임피던스매칭 및 차폐용 절연필름이 인출되는 단계(S121)와, 상기 단계(S121)에 의해 임피던스매칭 및 차폐용 절연필름이 차폐용절연필름권취롤로부터 인출되면서 이송되면, 제어부의 제어에 의해 개폐밸브가 개방되는 것에 대응되게 접착제저장부로부터 공급되는 접착제가 임피던스매칭 및 차폐용 절연필름의 일면에 도포되는 단계(S122)와, 상기 단계(S122)에 의해 이송중인 임피던스매칭 및 차폐용 절연필름의 일면에 접착제가 도포되면, 알루미늄권취롤에 권취되어 알루미늄인출용구동모터가 제어부에 의해 구동하는 것에 의해 접착제 타면측으로 박판의 알루미늄이 인출되어 부착되는 단계(S123)로 구성된 것을 특징으로 하는 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법.
The method of claim 1,
The impedance matching and electromagnetic shielding film manufacturing step (S120), the step of winding the insulating film for impedance matching and shielding by the drive motor is driven by the control unit is wound on the shielding film winding roll (S121), When the impedance matching and the shielding insulating film are drawn out from the shielding insulating film winding roll by the step (S121) and transferred, the adhesive supplied from the adhesive storing unit corresponds to the opening and closing valve under the control of the controller. And applying an adhesive to one surface of the impedance matching and shielding insulating film being transported by the step (S122), and the surface of the insulating film for shielding (S122), and wound on an aluminum winding roll to drive the aluminum pull-out. Comprising the step (S123) that the thin aluminum is drawn out and attached to the other surface of the adhesive by the motor driven by the control unit Impedance matching and electromagnetic shielding method of producing a one-piece insulating film characterized.
제1항 또는 제3항에 있어서,
상기 임피던스매칭 및 전자파 차폐용 필름 제조단계(S120)에 의해 제조된 임피던스매칭 및 전자파 차폐용 필름의 접착제를 안정화시키기 위한 단계(S130)는, 50℃~70℃의 내부온도를 갖는 숙성실에서 24시간~48시간 동안 체류시키는 것을 특징으로 하는 임피던스매칭 및 전자파 차폐 일체형 절연필름의 제조방법.
The method according to claim 1 or 3,
Step (S130) for stabilizing the adhesive of the impedance matching and electromagnetic shielding film prepared by the impedance matching and electromagnetic shielding film manufacturing step (S120), 24 hours in a aging room having an internal temperature of 50 ℃ ~ 70 ℃ Impedance matching and electromagnetic shielding integrated insulating film, characterized in that for 48 hours to stay.
삭제delete 삭제delete
KR1020130013147A 2013-02-06 2013-02-06 Manufacturing method of impedance matching and one electromagnetic shielding type relationship limit film KR101285690B1 (en)