JPH0735047B2 - Building material using Japanese paper and its manufacturing method - Google Patents

Building material using Japanese paper and its manufacturing method

Info

Publication number
JPH0735047B2
JPH0735047B2 JP2954391A JP2954391A JPH0735047B2 JP H0735047 B2 JPH0735047 B2 JP H0735047B2 JP 2954391 A JP2954391 A JP 2954391A JP 2954391 A JP2954391 A JP 2954391A JP H0735047 B2 JPH0735047 B2 JP H0735047B2
Authority
JP
Japan
Prior art keywords
japanese paper
water
building material
resin
paper
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP2954391A
Other languages
Japanese (ja)
Other versions
JPH04261801A (en
Inventor
一智 小倉
Original Assignee
一智 小倉
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 一智 小倉 filed Critical 一智 小倉
Priority to JP2954391A priority Critical patent/JPH0735047B2/en
Publication of JPH04261801A publication Critical patent/JPH04261801A/en
Publication of JPH0735047B2 publication Critical patent/JPH0735047B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は、和紙の有する独特の美
感を利用した床材、壁材等の建材に関し、更に詳細に
は、我が国古来の和紙の持つ素朴で安らぎのある感覚を
建材に生かすべく、あくまで本物の和紙を用いて、これ
に適切な処理を施したものである。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to building materials such as flooring materials and wall materials that utilize the unique aesthetics of Japanese paper, and more specifically, to the building materials that have the rustic and peaceful feeling of ancient Japanese paper. In order to make the best use of it, only genuine Japanese paper is used, and this is appropriately processed.

【0002】[0002]

【従来の技術】和紙は、触感が柔らかく、温かいイメ−
ジを有するため、見る人に素朴感と安らぎを与え、建材
として秀れた素材であり、又、古来から用いられた日本
固有の紙であるため、それがもたらす独特の美感が日本
人の古来の感情に合致した雰囲気を有している。
2. Description of the Related Art Washi paper has a soft texture and a warm texture.
It is a material that is excellent as a building material because it gives the viewer a simple feeling and peace of mind, and because it is a unique Japanese paper that has been used since ancient times, the unique beauty that it brings is the ancient Japanese Have an atmosphere that matches the feelings of.

【0003】そこで、この和紙の持つ美感上のイメ−ジ
を利用して、従来、家具の一部に和紙をそのまま貼って
デザイン上の工夫としたり、壁の表面にそのまま貼っ
て、壁の触感の冷たさを改善したりする試みが為されて
いる。又、和紙そのものを使用するものではないが、塩
化ビニ−ル、ポリエチレン等の合成樹脂フィルムを用
い、その表面に手漉き和紙の模様、図柄を模して印刷し
て壁材として、和紙の美感を利用した例がある。
Therefore, by utilizing the aesthetic image of this paper, the paper is conventionally stuck on a part of the furniture as it is, or it is stuck on the wall surface as it is, and the texture of the wall is touched. Attempts have been made to improve the coldness of the. Also, although Japanese paper itself is not used, a synthetic resin film such as vinyl chloride, polyethylene, etc. is used, and the surface of the paper is made by imitating the patterns and patterns of handmade Japanese paper, and it is printed as a wall material to give it a beautiful appearance. There is an example of using it.

【0004】しかし、前者は、和紙をそのまま使用する
ので、ほこり付着等による汚れの問題や、水や摩耗に対
して物理的強度が極めて弱い等の欠点があった。後者
は、物理的強度等の問題は解決されているが、和紙その
ものでなくあくまで模造品であるため、和紙本来の素朴
さ等が失われ、本物指向の強い需要者の好みには不満足
なものであった。
However, since the former uses the Japanese paper as it is, it has drawbacks such as a problem of dirt due to dust adhesion and a very weak physical strength against water and abrasion. Although the latter has solved problems such as physical strength, it is not a washi itself but an imitation product, so the original simplicity of the washi is lost, and it is unsatisfactory to the taste of consumers who have a strong genuine orientation. Met.

【0005】[0005]

【発明が解決しようとする課題】本発明者は、この和紙
の建材への応用について鋭意研究を進めた結果、あくま
で本物の和紙の雰囲気を楽しもうとする需要者の要望に
応えるため、和紙の特性を捕えることで、下記の課題を
解決することに成功したものである。
DISCLOSURE OF THE INVENTION As a result of earnestly researching the application of this washi to building materials, the present inventor has been able to meet the demands of consumers who want to enjoy the atmosphere of genuine washi. By capturing the characteristics, we have succeeded in solving the following problems.

【0006】(a)高温多湿な夏には、吸湿により繊維
が膨潤して皺がより易く、一方、低温乾燥の冬には、繊
維が収縮して切れ易いという欠点を有すること、(b)
水がかかると破れ易く、又、擦過や摩擦によって引裂き
や摩耗等が起きやすく、物理的に脆弱さを有すること、
(c)繊維の間にホコリやタバコのヤニが付着し易く、
人の手が触れると汚れ易く、しかし、水によるふき掃除
ができず、清潔に保って置くことが困難であること、
(d)時を経ると共に退色や風化等によって和紙固有の
美感が失われ易いこと、等の問題を解決せんとするもの
である。
(A) In the hot and humid summer, the fibers swell due to moisture absorption and wrinkles are more likely to occur. On the other hand, in the cold and dry winter, the fibers tend to shrink and break easily. (B)
It is easy to tear when exposed to water, and it is easy to tear or wear due to abrasion or friction, and it has physical weakness.
(C) Dust or tobacco tar tends to adhere between the fibers,
It easily gets dirty when touched by human hands, but it cannot be wiped clean with water and it is difficult to keep it clean.
(D) It is intended to solve the problems that the aesthetics peculiar to Japanese paper tend to be lost due to fading or weathering over time.

【0007】[0007]

【課題を解決するための手段】本発明和紙を利用した建
材は、表面にフッ素樹脂、シリコ−ン樹脂、ボロン樹脂
よりなる群から選ばれた一又は二以上の溌水性塗料を施
し、且つ、外側に層を形成しないよう薄手にした艶消塗
料で繊維の壁孔を遮蔽した和紙を、建材基盤の上に接着
させて成る。
A construction material using the present invention Japanese paper is a surface coated with one or more repellent paints selected from the group consisting of fluororesin, silicone resin and boron resin, and It is made by adhering Washi paper, which is made by thinning the matte paint so as not to form a layer on the outside, of the fiber wall holes, onto the building material base.

【0008】その詳細を製法と共に説明する。先ず、木
材、タイル、モルタル、等の床材、壁材等の建材を構成
する素材で建材基盤を作成する。この基盤は、後述の和
紙を貼付するための基礎部材となるもので、床材、壁材
等の用途に合せて、大きさ、形状を決定し、床材の場合
は、木材、ベニヤ板の他に、弾性を有するビニ−ルシ−
トやプラスチック材等が含まれる。壁材には、セッコウ
ボ−ドや軽量発泡コンクリ−トが含まれる。和紙は、コ
ウゾ、ミツマタなどの靭皮繊維を原料とした手漉き紙が
望ましいが、この手漉き和紙のイメ−ジを保持するもの
なら機械漉きでも良い。そして、この和紙から、床材、
壁材に合う図柄、模様、色彩をデザインしたものを選択
し、前記建材基盤の大きさに切断する。当該和紙には、
栃木県烏山や、出雲、嵯峨野の和紙等が利用できる。
The details will be described together with the manufacturing method. First, a building material base is made of materials that constitute building materials such as floor materials such as wood, tiles, mortar, and wall materials. This base serves as a base member for sticking Japanese paper, which will be described later, and the size and shape are determined according to the application such as floor material and wall material. In the case of floor material, other than wood, plywood, etc. In addition, an elastic vinyl seal
And plastic materials are included. The wall material includes gypsum board and lightweight foam concrete. Washi paper is preferably handmade paper made from bast fibers such as Kozo and Mitsumata, but mechanical paper may be used as long as it retains the image of the handmade Washi paper. And from this Japanese paper, floor material,
Select a design that has a design, pattern, or color that matches the wall material, and cut into the size of the building material base. The Japanese paper is
Karasuyama, Tochigi prefecture, Japanese paper from Izumo and Sagano can be used.

【0009】(膨潤、軟化)次に、当該建材基盤及び和
紙が用意されたら、このうち和紙に対し、水又は溶剤を
噴霧させるか、又は、水又は溶剤内に和紙を浸漬させ
て、水又は溶剤成分を繊維内に吸収させ、繊維の軟化及
び膨潤を図る。当該水又は溶剤の選択は、基盤と和紙と
の接着性を考慮して選んだ接着剤に合せて、水又は溶剤
を選ぶ。親水性の接着剤の場合は水を用い、親油性の接
着剤の場合は、有機溶剤を選び、その有機溶剤には、エ
チレングリコ−ル、キシレン、トルエン、トリクロロエ
チレン、テトラクロロエチレン、エタノ−ル、ナフサ、
メタノ−ル等を挙げることができる。又、噴霧又は浸漬
の選択は、水の場合は噴霧が好ましいが、溶剤の場合は
作業者の健康上から1〜2分程度の浸漬が望ましい。
(Swelling, Softening) Next, when the building material base and Japanese paper are prepared, water or a solvent is sprayed on the Japanese paper, or the Japanese paper is immersed in water or a solvent to prepare water or water. The solvent component is absorbed into the fiber to soften and swell the fiber. The water or solvent is selected in accordance with the adhesive selected in consideration of the adhesiveness between the base and Japanese paper. Water is used in the case of hydrophilic adhesive, and an organic solvent is selected in the case of lipophilic adhesive.The organic solvent is ethylene glycol, xylene, toluene, trichloroethylene, tetrachloroethylene, ethanol, naphtha. ,
Examples thereof include methanol. Further, the selection of spraying or dipping is preferably spraying in the case of water, but is preferably 1-2 minutes in the case of a solvent from the viewpoint of the health of the operator.

【0010】この和紙を軟化、膨潤させるのは、以下の
理由による。即ち、和紙の繊維は、比較的短い繊維が絡
み合って荒い結合をしており、伸び及び収縮率が均一で
なく、吸湿すると皺が寄り、逆に、乾燥すると切断がお
こる。そこで、この水分又は溶剤の吸収により、接着に
先立って予め繊維を膨潤させて絡みを解し、繊維が伸び
た状態で基盤に接着させんとするもので、これにより、
後で伸び及び収縮が起きても、皺や切断が発生しない効
果がある。又、この水分又は溶剤の吸収は、繊維を軟化
させ、撓みによって基盤に対し和紙をなじませるので、
空気の巻き込みを防止して滑らかな張りとなり、且つ、
接着が完全となる。
The reason for softening and swelling this Japanese paper is as follows. That is, the fibers of the Japanese paper are relatively entangled with each other to form a rough bond, the elongation and shrinkage are not uniform, and wrinkles occur when moisture is absorbed, and conversely, cutting occurs when dried. Therefore, by absorbing this water or solvent, the fibers are swollen in advance prior to adhesion to untangle them, and the fibers are allowed to adhere to the substrate in a stretched state.
Even if elongation and contraction occur later, there is an effect that wrinkles and cutting do not occur. Also, the absorption of this moisture or solvent softens the fibers and causes the Washi paper to fit into the substrate due to bending,
Prevents entrapment of air and creates a smooth tension, and
Adhesion is perfect.

【0011】(加圧接着)そして、この膨潤、軟化させ
た和紙と前記基盤とを、互の接着に適した接着剤を、例
えば、酢酸ビニル、ウレタン、エポキシ等から選んで接
着を図る。その接着は、和紙を貼付した基盤に、無加熱
で約6kg/cm2 〜10kg/cm2 程度の圧力をプ
レス機により加え、接着剤の硬化及び溶剤の飛散を促し
つつ、6〜7時間程度保持する。無加熱としたのは、熱
を加えると伝熱部に収縮が起こり易いので、これを避け
るためである。すると、前記水又は溶剤により軟化した
繊維がプレス圧力により基盤に押圧され、それが接着剤
の硬化と共に基盤に固着されので、空気の巻き込みがな
く且つ皺のない状態で接着がなされる。
(Pressure Adhesion) Then, the swollen and softened Japanese paper and the substrate are adhered by selecting an adhesive suitable for mutual adhesion, for example, vinyl acetate, urethane or epoxy. The adhesive is a foundation was attached Japanese paper, about 6kg / cm 2 ~10kg / cm 2 about pressure applied by the press machine without heating, while encouraging the hardening and scattering of the solvent of the adhesive, about 6-7 hours Hold. The reason why the heating is not performed is to avoid the shrinkage of the heat transfer portion easily occurring when heat is applied. Then, the fibers softened by the water or the solvent are pressed against the base by the pressing pressure, and the fibers are fixed to the base as the adhesive hardens, so that the air is not entrapped and the bonding is performed without wrinkles.

【0012】次いで、上記加圧後の基盤を、室温で6時
間程度放置して養生させる。この養生により、繊維内に
残った水分が徐々に蒸散し、乾燥する。しかし、基盤が
乾燥した木材等の水分を吸収する力が強いものである場
合には、蒸散を待たずに吸水されるので、養生の必要は
ない。
Next, the substrate after pressurization is left to cure at room temperature for about 6 hours. By this curing, the water remaining in the fibers is gradually evaporated and dried. However, when the substrate has a strong ability to absorb moisture, such as dried wood, water is absorbed without waiting for evaporation, so that curing is not necessary.

【0013】(内部保護処理)次に、養生後の和紙の内
部保護に移る。即ち、和紙の繊維たるコウゾ、ミツマタ
等の靭皮繊維は、その表面に壁孔3aと呼ばれる気孔を
点在させており、そのままにしておくと、湿気、蒸気等
が存在した場合には、当該壁孔3aから湿気等が侵入す
るので(後述の溌水性塗料を施しても湿気は通過するの
で)、a)湿気を吸収した繊維が軟質化し、手や物が触
れた場合に、破れや、摩耗を起こし易く、b)湿気の吸
収及び放散により、繊維の膨張と収縮が繰返されて接着
力を弱め、剥離等の原因となる等の不都合を生じる。
(Internal Protection Treatment) Next, the internal protection of the Washi paper after curing will be described. That is, the bast fibers such as Kozo and Mitsumata, which are the fibers of Japanese paper, have pores called wall pores 3a scattered on the surface, and if left as they are, when moisture, steam, etc. are present, Since moisture or the like enters through the wall holes 3a (because the moisture will pass even if a water repellent coating described later is applied), a) the fibers that have absorbed the moisture become soft, and when the hand or an object touches it, tears, It is liable to be worn, and b) absorption and diffusion of moisture cause repeated expansion and contraction of fibers to weaken the adhesive force and cause peeling and other inconveniences.

【0014】そこで、この和紙の特性に従い、この壁孔
3aを遮蔽して、壁孔3aから湿気が侵入するのを防ぐ
為、a)和紙の繊維と剥離等を起こさない親和性の良い
樹脂であり、b)繊維の弾性を失わせないよう可尭性を
有する樹脂を選び、塗付又は含浸させる。当該樹脂に
は、アクリル樹脂、ビニ−ル樹脂、ウレタン樹脂等が挙
げられる。そして、当該樹脂を、その樹脂の性格でピカ
ピカの艶が出てしまい和紙の素朴さを失わせることがな
いよう艶消性の樹脂を選択し、且つ、それが繊維の外に
食み出して層をなすことがないように、充分薄めに塗付
又は含浸させる。この為には、予め和紙重量に対し必要
な樹脂の量を実験から求めて置き、割合を厳守して樹脂
を含浸させる等の手段をとることができる。
Therefore, according to the characteristics of this Japanese paper, in order to block the wall holes 3a and prevent moisture from entering through the wall holes 3a, a) a resin having a good affinity with the fibers of the Japanese paper and causing no separation or the like. Yes, b) A flexible resin is selected so as not to lose the elasticity of the fiber, and is applied or impregnated. Examples of the resin include acrylic resin, vinyl resin, urethane resin and the like. Then, the resin is selected as a matte resin so that the shiny luster of the resin does not occur and the rusticness of the Japanese paper is not lost, and the resin dries out to the outside of the fiber. It is applied or impregnated sufficiently thin so that it does not form a layer. For this purpose, it is possible to take measures such as placing the amount of resin necessary for the weight of Japanese paper in advance through experiments and impregnating the resin in a strict proportion.

【0015】(表面処理)次に、上記養生後の和紙の表
面に、フッ素樹脂、シリコ−ン樹脂、ボロン樹脂よりな
る群から選ばれた一又は二以上の成分からなる溌水性の
塗料をスプレ−等で塗付する。これら溌水性塗料は、粒
子状の樹脂が繊維間に充填され、樹脂と繊維との一種の
凝集作用で結合しており、接触角及び濡れの点から水分
を弾き、和紙の水に弱い欠点を解消する。又、摩擦抵抗
が非常に低いので、人が触れたり、物が当ったりして
も、摩耗や破れを避けることができ、且つ、ホコリ、タ
バコのヤニ等に対しても、その付着を防止して綺麗に保
つことができる。この粒子は、ミクロン単位の微粒子で
あるから、繊維間に埋没し、従って、繊維の触感は変ら
ず、サラサラした和紙の膚触りをそのまま保持してい
る。又、粒子状であり、膜を形成しないので、膜により
光の屈折でピカ、ピカして和紙のイメ−ジを喪失させて
しまう欠点を解消している。
(Surface treatment) Next, a water-repellent paint comprising one or more components selected from the group consisting of fluororesin, silicone resin and boron resin is sprayed on the surface of the above-mentioned cured Japanese paper. -Coat with etc. These water-repellent coatings are filled with a particulate resin between the fibers and are bonded by a kind of cohesive action between the resin and the fiber, repel water from the point of contact angle and wetting, and have the drawback of being weak against the water of Japanese paper. Resolve. Also, since the frictional resistance is extremely low, it is possible to avoid wear and tear even if a person touches or hits an object, and to prevent the adhesion of dust, tobacco tar, etc. And keep it clean. Since these particles are fine particles of a micron unit, they are embedded between the fibers, and therefore, the feel of the fibers does not change, and the silky feel of the washi paper is retained as it is. Further, since it is in the form of particles and does not form a film, the defect that the image is shiny due to the refraction of light by the film and the image of Japanese paper is lost is solved.

【0016】[0016]

【発明の効果】以上の構成に基づいて、本発明和紙を利
用した建材は、本物の和紙を利用して、その素朴さ、温
かさを建材に表現できると共に、従来の欠点である切
れ、破れ、摩耗等の物理的強度の弱さを、表面処理及び
内部保護により克服でき、建材として優れて使用に耐え
るものとなった。又、適切な表面処理により、ホコリや
ヤニが付着しにくくなると共に、わずかに付着しても、
水でふき掃除ができるので、いつも清潔で綺麗に保つ利
点がある。そして、表面処理及び内部保護を適切にした
ので、樹脂の塗付又は含浸によってもピカピカになって
和紙のイメ−ジを失う等の不都合が発生せず、又、触っ
た感覚もサラサラとした和紙の感覚を保持している。
EFFECTS OF THE INVENTION Based on the above constitution, the building material using the Japanese paper of the present invention can express the rusticness and warmth in the building material by using the genuine Japanese paper, and at the same time, the conventional drawbacks such as breaking and tearing, Weakness in physical strength such as abrasion could be overcome by surface treatment and internal protection, and it became excellent as a building material and durable. Also, with appropriate surface treatment, it becomes difficult for dust and tar to adhere, and even if it adheres slightly,
Since it can be wiped clean with water, it has the advantage of always keeping it clean. Since the surface treatment and internal protection were made appropriate, there is no inconvenience such as loss of the image of the washi paper even if it is applied or impregnated with the resin, and the touch feeling is also smooth. Holds a sense of.

【0017】[0017]

【実施例】床材用のベニヤ板を30×30×5mmの大
きさに切断したもの10枚を準備した。一方、和紙とし
て、栃木県烏山産のものを用意し、これを上記床板の大
きさに合うよう切断した。この和紙にスプレ−で水を噴
霧させ、繊維を軟化、膨潤させた。同時に、床板の表面
に水溶性の接着剤、酢酸ビニ−ルを塗付し、その上に上
記軟化、膨潤させた和紙を貼付した。これを、プレス機
にかけて5kg/cm2 の圧力を加えて接着させ、6時
間養生した。次に、艶消性のアクリル樹脂をキシレンに
溶かし、和紙40g/cm2 に対し、溶剤20g/cm
2 の割合で浸漬させて、繊維に内部保護樹脂を含浸させ
た。放置して乾燥させ、これに4フッ化エチレンをスプ
レ−ガンで噴霧して繊維間に凝集結合させた。その結
果、和紙の素朴で温かい感覚が表現でき、且つ、耐水性
に秀れ、汚れやホコリの付着の少ない秀れた床材が得ら
れた。
EXAMPLE Ten veneer boards for flooring were prepared by cutting them into a size of 30 × 30 × 5 mm. On the other hand, Japanese paper produced in Karasuyama, Tochigi Prefecture was prepared and cut to fit the size of the floorboard. The Japanese paper was sprayed with water to soften and swell the fibers. At the same time, a water-soluble adhesive, vinyl acetate, was applied to the surface of the floorboard, and the softened and swollen Japanese paper was applied thereon. This was put on a press machine to apply a pressure of 5 kg / cm 2 for adhesion and cured for 6 hours. Next, a matt acrylic resin is dissolved in xylene, and the solvent is 20 g / cm 2 against 40 g / cm 2 of Japanese paper.
The fiber was impregnated with the internal protective resin by immersing it in the ratio of 2 . It was left to dry and then tetrafluoroethylene was sprayed with a spray gun to cause cohesive bonding between the fibers. As a result, it was possible to obtain an excellent flooring material capable of expressing the rustic and warm feeling of Japanese paper, having excellent water resistance, and having little dirt or dust adhesion.

【図面の簡単な説明】[Brief description of drawings]

【図1】本発明建材の一部切欠斜視図である。FIG. 1 is a partially cutaway perspective view of a building material of the present invention.

【図2】本発明建材の一部縦断側面図である。FIG. 2 is a partially longitudinal side view of the building material of the present invention.

【図3】和紙の繊維を拡大した斜視図である。FIG. 3 is an enlarged perspective view of fibers of Japanese paper.

【符号の説明】[Explanation of symbols]

1 建材基盤 2 接着剤 3 和紙 3a 壁孔 4 溌水性塗料 1 Building material base 2 Adhesive 3 Washi 3a Wall hole 4 Water-repellent paint

Claims (2)

【特許請求の範囲】[Claims] 【請求項1】 表面にフッ素樹脂、シリコ−ン樹脂、ボ
ロン樹脂よりなる群から選ばれた一又は二以上の溌水性
塗料を施し、且つ、外側に層を形成しないよう薄手にし
た艶消塗料で繊維の壁孔を遮蔽した和紙を、建材基盤の
上に接着させて成る和紙を利用した建材。
1. A matte coating which has one or two or more water-repellent coatings selected from the group consisting of fluororesin, silicone resin, and boron resin on the surface and is thin so as not to form a layer on the outside. A building material that uses Japanese paper that is made by adhering the Japanese paper with the fiber wall holes blocked on it on the building material base.
【請求項2】 絡合した和紙繊維に水又は溶剤を噴霧又
は浸漬させて膨潤、軟化させた後、床板、壁材等の建材
基盤に接着剤で加圧下に接着させ、養生後、当該和紙繊
維の壁孔を外側に層を形成しないよう薄手にした艶消し
塗料で遮蔽し、更に、その表面にフッ素樹脂、シリコ−
ン樹脂、ボロン樹脂よりなる群から選ばれた一又は二以
上の溌水性塗料を施したことを特徴とする和紙を利用し
た建材の製造法。
2. The entangled Japanese paper fibers are sprayed or dipped with water or a solvent to swell and soften them, and then adhered to a building material base such as floor boards and wall materials under pressure with an adhesive, and after curing, the Japanese paper The wall holes of the fiber are shielded with a thin matte paint so as not to form a layer on the outside, and on the surface, fluororesin, silicone
A method for producing a building material using Japanese paper, characterized in that one or more water-repellent paints selected from the group consisting of resin and boron resin are applied.
JP2954391A 1991-01-30 1991-01-30 Building material using Japanese paper and its manufacturing method Expired - Fee Related JPH0735047B2 (en)