JP5509665B2 - 高強度厚肉熱延鋼板の巻き取り装置および巻き取り方法 - Google Patents
高強度厚肉熱延鋼板の巻き取り装置および巻き取り方法 Download PDFInfo
- Publication number
- JP5509665B2 JP5509665B2 JP2009102727A JP2009102727A JP5509665B2 JP 5509665 B2 JP5509665 B2 JP 5509665B2 JP 2009102727 A JP2009102727 A JP 2009102727A JP 2009102727 A JP2009102727 A JP 2009102727A JP 5509665 B2 JP5509665 B2 JP 5509665B2
- Authority
- JP
- Japan
- Prior art keywords
- coil
- winding
- rolled steel
- hot
- steel sheet
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Description
[1]コイラー装置と該コイラー装置からコイルを抜き出すコイルカーを備える高強度
厚肉熱延鋼板の巻き取り装置であって、該コイルカーは、コイル軸心方向と平行
な方向に中心軸を有する、コイルを支持するための2本のクレードルロールを備
え、かつ2本のクレードルロールの軸心間距離を可変にする手段を備えているこ
とを特徴とする、高強度厚肉熱延鋼板の巻き取り装置。
[2][1]に記載の高強度厚肉熱延鋼板の巻き取り装置を用いた巻き取り方法であっ
て、2本のクレードルロールの軸心間距離を、鋼種、巻き取り温度、コイル重
量、板厚、板幅に応じて設定したことを特徴とする、高強度厚肉熱延鋼板の巻き
取り方法。
なお、本発明では高強度の定義はAPI規格にてX65以上、厚肉熱延鋼板は製品厚にて15mm以上のものを対象としている。
本発明者らは、この高強度厚肉熱延鋼板コイルのスプリングバックによるコイル浮き上がりの問題を解決するための技術について鋭意検討を重ねた結果、コイル自重によって発生する曲げモーメントを大きくすることにより、コイルの浮き上がり、巻き緩みを抑制した巻き取りが可能であることを見出し、本発明を完成した。
コイラー装置により熱延鋼板1の先端部を巻き取るにあたっては、ピンチロール3、マンドレル7、ラッパーロール5などの各ロールの周速は、熱延鋼板1の厚さや硬さ(強度)などに応じて、熱延鋼板1の搬送速度に対し、10〜30%のリード率をもたせた値、すなわち、10〜30%速い速度に制御している。この際、マンドレル7、ラッパーロール5のリード率は、ピンチロール3のリード率以上としている。
なお、図3ではラッパーロールの数は4基としているが、3基のものもあり、熱延鋼板のコイラー装置では一般的には3〜4基である。
なお、熱延鋼板の尾端部がコイラーの手前20m程度に来ると、巻き取り終了に向けて、熱延鋼板の搬送速度(巻き取り速度)は減速される。
なお、クレードルロール8は、コイルカーに同径のものが2本備えられており、コイルカーがコイルの下に待機したときに、2本のクレードルロールの軸はコイル軸心(マンドレル軸心)と平行になっている。
Mp=(h2w/4)・σy (1)
(1)式において、hは板厚、wは板幅、σyは材料の降伏応力である。
図1および図2において、コイラー装置は図3に示されたものと同じである。9はコイルカーである。図ではコイル下に待機して、上昇後のコイルカーが示されている。コイルカー9には、前述したように、コイルカー9が上昇してコイル1に当接する2本の同径のクレードルロール8がコイル中心軸方向と平行に設けられている。
クレードルロール8はコイルカー9上で水平方向に移動可能な手段が設けられており、2本のクレードルロールは、マンドレル7の回転軸心に対して対称に近接離反が可能な構造となっている。図1および図2において、Lは2本のクレードルロールの軸心間距離を示している。
対象とした材料はAPI規格X80グレードであり、厚み250mm、幅1200、1500、1800mm、重量24トン、30トンのスラブを熱間圧延ラインの粗圧延工程、仕上圧延工程を経て厚み19、22、25.4mmに仕上げ、冷却テーブル上にて520℃まで冷却したのちにコイラー装置により巻き取った。
本発明の実施例においては、クレードルロール間距離Lは、550〜950mmの間で可変であり、L=550、650、750、850、950mmの5水準に設定した。比較例でのLは、従来の巻き取り装置でのクレードルロール軸心間距離と同程度の550mmに固定した。
表1に本実施例での評価結果を示す。
クレードルロール間距離Lを、従来の巻き取り装置でのクレードルロール軸心間距離と同程度の550mmに固定とした場合、以下に示すように比較例の一部にはコイルが浮き上がり、コイル抜き出しができなかった。
これに対し、本発明にてクレードルロール間距離Lを適切に設定した場合には、比較例ではコイル浮き上がりが発生していた鋼板コイルにおいても、コイルの浮き上がりが抑制できることが確認できた。
2:エプロン
3a、3b:ピンチロール
4:スロートガイド
5a〜5d:ラッパーロール
6:ストリップガイド
7:マンドレル
8:クレードルロール
9:コイルカー
Claims (2)
- コイラー装置と該コイラー装置からコイルを抜き出すコイルカーを備える高強度厚肉熱延鋼板の巻き取り装置であって、該コイルカーは、コイル軸心方向と平行な方向に中心軸を有する、コイルを支持するための2本のクレードルロールを備え、かつ2本のクレードルロールの軸心間距離を可変にする手段を備えていることを特徴とする、高強度厚肉熱延鋼板の巻き取り装置。
- 請求項1に記載の高強度厚肉熱延鋼板の巻き取り装置を用いた巻き取り方法であって、2本のクレードルロールの軸心間距離を、鋼種、巻き取り温度、コイル重量、板厚、板幅に応じて設定したことを特徴とする、高強度厚肉熱延鋼板の巻き取り方法。