DE1900466A1 - Salzbad zur Entzunderung von Metallen,insbesondere von Eisen und Eisenlegierungen - Google Patents
Salzbad zur Entzunderung von Metallen,insbesondere von Eisen und EisenlegierungenInfo
- Publication number
- DE1900466A1 DE1900466A1 DE19691900466 DE1900466A DE1900466A1 DE 1900466 A1 DE1900466 A1 DE 1900466A1 DE 19691900466 DE19691900466 DE 19691900466 DE 1900466 A DE1900466 A DE 1900466A DE 1900466 A1 DE1900466 A1 DE 1900466A1
- Authority
- DE
- Germany
- Prior art keywords
- iron
- salt bath
- metals
- descaling
- nitrate
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Description
Pafentanwülte
6 Frci-.k'uit α. M.
Mi;ielweg 12
Mi;ielweg 12
KOLENE Corporation 12b9O, Westwood Avenue, Detroit] Michigan 4Ö223, U.S.A.
Salzbad zur Entzunderung von Metallen, insbesondere von Eisen
und Eisenlegierungen.
Die Erfindung bezieht sich auf ein Salzbad, das zur Entzunderung von Metallen, insbesondere von Eisen und Eisenlegierungen, bestimmt
ist.
i)ei der Bearbeitung von Werkstücken aus derartigen Metallen ist
es häufig notwendig, das Material zwischen den einzelnen Bec.rbeitungsvorgängen
zu erhitzen. Diese Wärmebehandlungen werden häufig in einer oxydierenden Atmosphäre durchgeführt, wodurch
sich eine Oxidschicht an der Oberfläche der Metalle bildet. In den meisten Fällen ist es notwendig, diese Oxidschicht von der
Metalloberfläche zu entfernen.
Ds ist bekannt, die Entfernung der Oxidschichten in einem sauren Medium durchzuführen. In manchen Fällen ist es jeodch schwierig
oder unmöglich, durch eine derartige Säurebehandlung die Oxidrfchicht
zu' entfernen oder die Zeit ist zu lang, um diese Säurebehandlung durchzuführen.
i-js sind verschiedene Vorschläge bekannt, um die Entzunderung bei
uerartigen Metallen durchzuführen. Beispielsweise sind Behandlungsverfahren bekannt, wie sie auch in den amerikanischen
Λι-enten 3 321 026 und 3 254 011 beschrieben sind. Diese Patente
beziehen sich auf wässrige Lösungen, die aus einem Gemisch von
Kaliumhydroxid und Kaliumnitrat bestehen. In diesen Patenten
wird weiterhin angegeben, dass diese Salze geeignet sind, Titan i.ml rostfreien Stahl zu behandeln. Diese wässrigen Lösungen
von kaliumhydroxid und Kaliumnitrat sind jedoch in gewissen
- 2 909835/1268
Fällen nicht anwendbar, da sie das Metall selbst angreifen.
Vorliegende Erfindung verbessert derartige Bäder dadurch, dass nicht die reinen Salze verwendet werden, sondern solche
Salze, die Hydratwasser enthalten.
Die Erfindung bezieht sich insbesondere auf Bäder mit einer wässrigen Lösung von Kaliumhydroxid und Kaliumnitrat, die
Verwendung finden zur Desoxydierung von Titan, r&stfreiem
Stahl und anderen Metallen, bei denen es schwierig ist, die fe Oxidschicht von der Oberfläche zu entfernen. Vorzugsweise
werden Gehalte zwischen 5 und 30 % Kaliumnitrat eingesetzt.
Die Herstellung dieses Mischsalzes erfolgt in der Weise, dass Xaliumhydroxid, Kaliumnitrat und eine gewisse Wassermenge
über dem Temperaturpunkt erhitzt werden, bei dem sie schmelzen. Sie werden für eine gewisse Zeit auf dieser Temperatur gehalten,
damit eine einwandfreie Mischung zwischen diesen Grundstoffen erreicht wird. Der Anteil von Wasser in der
Mischung ist abhängig von der Zeit und der Temperatur, je höher die Temperatur und je länger die Zeit andauern, je .
weniger Wasser verbleibt in diesem Salzgemisch.
" Wenn diese Mischung die gewünschte Zusammensetzung erreicht hat,
wird sie gekühlt, wobei sich eine einheitliche Mischung von Kaliumhydroxid, Kaliumnitrat und Wasser ergibt. Dieses Produkt
besitzt die Form von Flocken.
909835/1268
Claims (3)
1. Salzbad zur Entzunderung von Metallen, insbesondere
von Eisen und Eisenlegierungen, dadurch gekennzeichnet dass es aus einer Lösung von Alkalihydroxid ,eines
Nitrats und aus Hydratwasser besteht.
2. Salzbad nach Anspruch 1, dadurch gekennzeichnet, dass dass das Alkalihydroxid aus Natrium- oder Kaliumhydroxid
besteht.
3. Salzbad nach Anspruch 2, dadurch gekennzeichnet, dass
das Nitratsalz aus einem Alkalinitrat besteht.
k. Salzbad nach den Ansprüchen 1 bis 3, dadurch gekennzeichnet,
dass es aus 60 bis 90 fo Kaliumhydroxid,
5 bis 30 % Kaliumnitrat und 5 bis 20 <fo Wasser besteht.
2.I.1969
Schn/Bi
Schn/Bi
909835/1268