CN105906892A - Method for improving rubber air tightness - Google Patents

Method for improving rubber air tightness Download PDF

Info

Publication number
CN105906892A
CN105906892A CN201610449643.3A CN201610449643A CN105906892A CN 105906892 A CN105906892 A CN 105906892A CN 201610449643 A CN201610449643 A CN 201610449643A CN 105906892 A CN105906892 A CN 105906892A
Authority
CN
China
Prior art keywords
rubber
parts
air tightness
kaolin
rubber air
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201610449643.3A
Other languages
Chinese (zh)
Inventor
莫海燕
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
LIUZHOU YINGHANG AUTOMOBILE ACCESSORY Co Ltd
Original Assignee
LIUZHOU YINGHANG AUTOMOBILE ACCESSORY Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by LIUZHOU YINGHANG AUTOMOBILE ACCESSORY Co Ltd filed Critical LIUZHOU YINGHANG AUTOMOBILE ACCESSORY Co Ltd
Priority to CN201610449643.3A priority Critical patent/CN105906892A/en
Publication of CN105906892A publication Critical patent/CN105906892A/en
Pending legal-status Critical Current

Abstract

The invention discloses a method for improving the rubber air tightness, and belongs to the technical field of rubber component manufacturing. The method comprises the steps that additives accounting for 15-20% of the mass of rubber are added in the rubber preparation process, wherein the additives are prepared from, by weight, 15-20 parts of cyanate ester resin, 10-15 parts of acrylic resin, 6-10 parts of sodium tripolyphosphate and 0.1-0.2 part of kaolin. The additives prepared from the cyanate ester resin, the acrylic resin, the sodium tripolyphosphate and the kaolin on the basis of the specific proportion are added into rubber, and therefore the rubber air tightness is improved.

Description

The method improving rubber air tightness
Technical field
The invention belongs to rubber accessory manufacturing technology field, particularly relate to a kind of method improving rubber air tightness.
Background technology
The method improving rubber air tightness is mainly made up of inner glue layer and outer glue-line, and it is applicable to compressed air, automobile parts shop and pneumatic (air pressure) instrument, and water and the conveying of non-corrosive liquid, is widely used in industry, building industry, agricultural etc. and leads.
Summary of the invention
The technical problem to be solved is to provide a kind of method improving rubber air tightness that air-tightness is good.
In order to solve above-mentioned technical problem, the technical solution adopted in the present invention is:
It is in the preparation process of rubber, is added into the additive accounting for described rubber quality 15%~20%;Wherein, described additive is counted by weight, is made up of cyanate ester resin 15 parts~20 parts, acrylic resin 10 parts~15 parts, sodium tripolyphosphate 6 parts~10 parts, Kaolin 0.1 part~0.2 part.
Owing to using technique scheme, there is advantages that
The present invention is mainly by adding the additive being made up of cyanate ester resin, acrylic resin, sodium tripolyphosphate, Kaolin of special ratios in rubber, thus improves the air-tightness of rubber.
Detailed description of the invention
Below in conjunction with instantiation, the invention will be further described:
Embodiment 1
It is in the preparation process of rubber that the present embodiment improves the method for rubber air tightness, is added into the additive accounting for described rubber quality 15%;Wherein, described additive is counted by weight, is made up of cyanate ester resin 15 parts, acrylic resin 15 parts, sodium tripolyphosphate 7 parts, Kaolin 0.1 part.
The air transmission coefficient of the rubber that the present embodiment prepares is 1.346E-13cm3.cm/cm2.s.Pa。
Embodiment 2
It is in the preparation process of rubber that the present embodiment improves the method for rubber air tightness, is added into the additive accounting for described rubber quality 17%;Wherein, described additive is counted by weight, is made up of cyanate ester resin 20 parts, acrylic resin 10 parts, sodium tripolyphosphate 6 parts, Kaolin 0.15 part.
The air transmission coefficient of the rubber that the present embodiment prepares is 1.345E-13cm3.cm/cm2.s.Pa。
Embodiment 3
It is in the preparation process of rubber that the present embodiment improves the method for rubber air tightness, is added into the additive accounting for described rubber quality 20%;Wherein, described additive is counted by weight, is made up of cyanate ester resin 17 parts, acrylic resin 12 parts, sodium tripolyphosphate 10 parts, Kaolin 0.2 part.
The air transmission coefficient of the rubber that the present embodiment prepares is 1.344E-13cm3.cm/cm2.s.Pa。

Claims (1)

1. the method improving rubber air tightness, it is characterised in that:
In the preparation process of rubber, it is added into the additive accounting for described rubber quality 15%~20%;Wherein, described additive is counted by weight, is made up of cyanate ester resin 15 parts~20 parts, acrylic resin 10 parts~15 parts, sodium tripolyphosphate 6 parts~10 parts, Kaolin 0.1 part~0.2 part.
CN201610449643.3A 2016-06-21 2016-06-21 Method for improving rubber air tightness Pending CN105906892A (en)