CN105506196A - Preparation process for pig skin top layer instep leather free of chrome tanning - Google Patents

Preparation process for pig skin top layer instep leather free of chrome tanning Download PDF

Info

Publication number
CN105506196A
CN105506196A CN201610050180.3A CN201610050180A CN105506196A CN 105506196 A CN105506196 A CN 105506196A CN 201610050180 A CN201610050180 A CN 201610050180A CN 105506196 A CN105506196 A CN 105506196A
Authority
CN
China
Prior art keywords
tanning
add
agent
preparation technology
retanning
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201610050180.3A
Other languages
Chinese (zh)
Other versions
CN105506196B (en
Inventor
钱世峰
石益英
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Haining Home Textile Industrial Base Investment Development Co ltd
Original Assignee
Huzhou Great Wall Leather Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Huzhou Great Wall Leather Co Ltd filed Critical Huzhou Great Wall Leather Co Ltd
Priority to CN201610050180.3A priority Critical patent/CN105506196B/en
Publication of CN105506196A publication Critical patent/CN105506196A/en
Application granted granted Critical
Publication of CN105506196B publication Critical patent/CN105506196B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention belongs to the field of instep leather preparation processes, and particularly relates to a preparation process for pig skin top layer instep leather free of chrome tanning. The preparation process comprises the following steps that from pickled skin scytoblastema, the addition quantity of additives in all the procedures is based on the mass of pickled skin, and pickling and softening, main tanning, degreasing and softening, retanning, water extruding and neutralizing, dyeing and stuffing and staking and spouting are included. The preparation process for the pig skin top layer instep leather free of chrome tanning has the advantages that the steps are simple, preparation efficiency is high, the requirement of the preparation process for equipment is low, energy saving and environment friendliness are achieved, and the prepared instep leather is resistant to wear and high temperature, full and soft.

Description

A kind of without chrome tanning pigskin head layer upper leather preparation technology
Technical field
The invention belongs to upper leather preparation technology field, particularly relate to a kind of without chrome tanning pigskin head layer upper leather preparation technology.
Background technology
Curriery is the important traditional light industry of China, is also one of comparatively serious industry of blowdown.Traditional leather many employings chromium makes tanning agent, the chrome tanned leather that processing obtains has high temperature resistant, Heat stability is good, leather body is plentiful, soft advantage, but because the heavy metal contamination that chromium ore resource is limited and chrome tanning produces, in people's pay attention to day by day living environment, pay close attention to the today using environmental protection leather, development becomes inexorable trend without chrome tanning leather.
The Chinese invention patent that patent publication No. is CN101225450A, publication date is 2008.07.23 discloses the chrome-free tanning production technique of a kind of goat skin gloves leather, include following step, softening → pickling → organic phosphine tanning → be oxidized → take horse to leave standstill → water squeezing stretching, extension → shaving → washing → degreasing, rinsing → washing → using brother chemicals → washing, then chrome tanning subsequent technique routinely carries out.
But it is complicated to there is tanning step in the production technique of this invention, and efficiency is low, and the glove leather of tanning is of poor quality, plentiful not, problem soft not.
Summary of the invention
The object of this invention is to provide a kind of without chrome tanning pigskin head layer upper leather preparation technology, it is simple that it has step, and preparation efficiency is high, and the upper leather preparing gained is wear-resisting, high temperature resistant, plentiful, soft advantage.
The technical scheme that the present invention overcomes the above problems employing is: a kind of without chrome tanning pigskin head layer upper leather preparation technology, comprise the following steps (from sour skin scytoblastema, the addition of each operation additive with the quality of sour skin for benchmark): pickling eases back, main tanning, degreasing eases back, retanning, water squeezing neutralizes, dyeing and fat-liquoring and draw soft whitewashing, the described pickling liquor ratio in step that eases back is 200%, add the sulfuric acid of 1.0-1.2%, the Industrial Salt of 10-12%, pH is 1.8-2.3, temperature is 25-28 DEG C, the time of easing back is 120-150min, chrome-free tanning agent is adopted in described main tanning step, comprise aluminum tanning agent and glutaraldehyde aldehyde tanning agent, pH scope divides three phases, early stage is 3.2-3.3, sodium formiate and sodium bicarbonate adjustment is added by first time, mid-term is 3.5-3.6, add sodium formiate by second time to regulate, later stage is 4.0-4.5, add sodium bicarbonate by second time to regulate, temperature is 33-35 DEG C, the described degreasing liquor ratio in step that eases back is 100%, add the oxalic acid of 1.0-1.2% and the grease-removing agent of 1.0-1.5%, pH is 3.2-3.3, temperature is 45-48 DEG C, the time of easing back is 60-65min, composite tanning agent is adopted in described retanning step, liquor ratio is 100%, pH is 4.2-4.3, retanning temperature is 32-35 DEG C, the neutralizing agent adopted in described water squeezing neutralization procedure is sodium formiate and sodium bicarbonate, pH is 5.8-6.0, temperature is 30-32 DEG C, in and the time be 90-100min, cationic fat liquor is adopted in described dyeing and fat-liquoring step, pH is 3.8-4.0, temperature is 52-55 DEG C, described drawing in soft whitewashing step draws soft operation and whitewashing operation to hocket, comprise altogether 3-4 group and draw soft whitewashing operation.It is simple that the preparation technology of the layer of pigskin head described in this setting upper leather has step, and preparation efficiency is high, the advantage of the low and energy-conserving and environment-protective of the requirement of preparation process to equipment.
Preferred technical scheme is further: before adding described tanning agent, first add sodium formiate in described main tanning step, sodium bicarbonate and phospho-glycerol three ester, stir 60-70min, the amount adding described aluminum tanning agent is successively 2.0-2.2%, described glutaraldehyde tanning agent is 6.0-6.5%, the amount of described glutaraldehyde tanning agent evenly divides three parts, successively add respectively for three times, and constantly stir, add other compositions of becoming owner of in tanning afterwards again, add sodium formiate successively, antioxidant, tannin, iron powder, mould inhibitor and sodium bicarbonate, the scope of the amount of described main tanning ancillary component is 8.0-12.0%, finally stir 300-500min.Each inherent regulation after in before the pH of main tanning step described in this setting, improves the effect of described main tanning, makes the leather of tanning more plentiful, soft.
Preferred technical scheme is further: described mould inhibitor comprises TCMTB(2-thiocyanogen methyl sulfuration benzothiazole) and OIT(octylisothiazolinone), the mass ratio of described TCMTB and described OIT consumption is 1:1-1:2.
Preferred technical scheme is further: the amount that described second time sodium bicarbonate adds is 1.5-2.0%, is divided into five times and adds, every minor tick 30-35min.
Further preferred technical scheme is: carry out after described main tanning step that drum takes that horse leaves standstill successively, setting-out, get rid of soft and shaving deburring step, the bilayer thickness controlling described leather in described shaving step is 2.0-2.4mm.
Further preferred technical scheme is: the composite tanning agent adopted in described retanning step comprises acrylate resin tanning agent, the Caesalpinia spinosaKuntze vegetable tanning agent of improvement and glutaraldehyde tanning agent, the amount that described acrylate resin tanning agent adds is 2.0-2.5%, the amount that the Caesalpinia spinosaKuntze vegetable tanning agent of described improvement adds is 2.2-2.5%, add rear stirring 90-100min, add retanning ancillary component afterwards, then stir 250-300min.
Preferred technical scheme is further: described retanning ancillary component comprises toughner, surfactivity defrosting compound and retanning filler, and the sodium bicarbonate finally adding 1.0-1.2% regulates pH to be 4.2-4.3, and the amount that described retanning ancillary component adds is 6.0-8.5%.
Preferred technical scheme is further: add the vulcanization accelerator for improving leather machine performance in described water squeezing neutralization procedure, the amount added is 1.0-1.2%.
Preferred technical scheme is further: described dyeing and fat-liquoring step is divided into dyeing process and stuffing operation, dyestuff, diffusant, migration inhibitor and surface active agent is added in described dyeing process, the total amount that described diffusant, migration inhibitor and surface active agent add is 7.0-9.5%, the fatting agent added in described stuffing operation comprises sulfonation synthetic oil and sulfited fish oil, the total amount added is 6.0-8.0%, finally regulates pH and stirs.
Preferred technical scheme is further: described in described dyeing and fat-liquoring step, dyeing process and stuffing operation add the formic acid of 1.5-1.8% as neutralizing agent after all completing, and adjustment pH is 3.9-4.0, finally stirs, and churning time is 100-120min.
The invention provides a kind of without chrome tanning pigskin head layer upper leather preparation technology, it is simple that it has step, and preparation efficiency is high, and preparation process is low for equipment requirements, energy-conserving and environment-protective, and the upper leather preparing gained is wear-resisting, high temperature resistant, plentiful, soft advantage.
Embodiment
The following stated is only preferred embodiment of the present invention, non-ly limits scope of the present invention.
Embodiment: a kind of without chrome tanning pigskin head layer upper leather preparation technology, comprise the following steps (from sour skin scytoblastema, the addition of each operation additive with the quality of sour skin for benchmark): pickling eases back, main tanning, degreasing ease back, retanning, water squeezing neutralization, dyeing and fat-liquoring and draw soft whitewashing, the following detailed description of the specific embodiment of the present invention:
Operation consumption materials temperature-time remarks
Pickling eases back 10% Industrial Salt, 25 DEG C of liquor ratios 200%
1.0% sulfuric acid 120minpH1.8
Main tanning 1.0% sodium formiate
0.5% sodium bicarbonate 30minpH3.0
0.5% phospho-glycerol three ester 30min
2.0% aluminum tanning agent 60min
2.0% glutaraldehyde tanning agent 60min
2.0% glutaraldehyde tanning agent 60min
2.0% glutaraldehyde tanning agent 90min
1.0% sodium formiate 30minpH3.5
1.0% antioxidant 10min
2.0% tannin 30min
2.0% tannin 30min
2.0% tannin 90min
0.2% iron powder
0.1% mould inhibitor 30min(TCMTB:OIT=1:1)
1.5% sodium bicarbonate 30 × 5minpH4.0
(be warming up to 35 DEG C, stir 300min, then stop drum and spend the night)
Go out drum and take that horse leaves standstill, setting-out gets rid of soft, shaving deburring, bilayer thickness 2.0mm
Degreasing eases back 1.0% oxalic acid, 45 DEG C of liquor ratios 100%
1.0% grease-removing agent 60minpH3.2
25 DEG C of washing 30min
Retanning 2.0% acrylic tanning agent 32 DEG C of 30min liquor ratios 100%
2.0% Caesalpinia spinosaKuntze tanning agent 30min
2.0% glutaraldehyde tanning agent 60min
2.0% toughner 30min
1.0% active defrosting compound 40min
2.0% retanning filler 60min
1.0% sodium bicarbonate 30 × 3minpH4.2
With 1.0% vulcanization accelerator 30 DEG C in water squeezing
1.0% sodium formiate
2.0% sodium bicarbonate 90minpH5.8
25 DEG C of washing 30min
Dyeing and fat-liquoring dyestuff 52 DEG C
1.0% diffusant
2.0% migration inhibitor
4.0% surface active agent 45min
3.0% sulfonation synthetic oil
2.0% sulfited fish oil 50min
1.5% formic acid 30 × 2minpH3.8
Cooling take out, hang dry in the air get rid of soft, toggling deburring, continuous three times whitewashing draw soft, deburring dipping put in storage
Above embodiments of the present invention are explained in detail, but the invention is not restricted to above-mentioned embodiment, in the ken that described technical field those of ordinary skill possesses, various amendment can also be made under the prerequisite not departing from present inventive concept.These are all not creative amendments, as long as be all subject to the protection of patent law in right of the present invention.

Claims (10)

1. one kind without chrome tanning pigskin head layer upper leather preparation technology, comprise the following steps (from sour skin scytoblastema, the addition of each operation additive with the quality of sour skin for benchmark): pickling eases back, main tanning, degreasing eases back, retanning, water squeezing neutralizes, dyeing and fat-liquoring and draw soft whitewashing, it is characterized in that: the described pickling liquor ratio in step that eases back is 200%, add the sulfuric acid of 1.0-1.2%, the Industrial Salt of 10-12%, pH is 1.8-2.3, temperature is 25-28 DEG C, the time of easing back is 120-150min, chrome-free tanning agent is adopted in described main tanning step, comprise aluminum tanning agent and glutaraldehyde tanning agent, pH scope divides three phases, early stage is 3.2-3.3, sodium formiate and sodium bicarbonate adjustment is added by first time, mid-term is 3.5-3.6, add sodium formiate by second time to regulate, later stage is 4.0-4.5, add sodium bicarbonate by second time to regulate, temperature is 33-34 DEG C, the described degreasing liquor ratio in step that eases back is 100%, add the oxalic acid of 1.0-1.2% and the grease-removing agent of 1.0-1.5%, pH is 3.2-3.3, temperature is 45-48 DEG C, the time of easing back is 60-65min, composite tanning agent is adopted in described retanning step, liquor ratio is 100%, pH is 4.2-4.3, retanning temperature is 32-35 DEG C, the neutralizing agent adopted in described water squeezing neutralization procedure is sodium formiate and sodium bicarbonate, pH is 5.8-6.0, temperature is 30-32 DEG C, in and the time be 90-100min, cationic fat liquor is adopted in described dyeing and fat-liquoring step, pH is 3.8-4.0, temperature is 52-55 DEG C, described drawing in soft whitewashing step draws soft operation and whitewashing operation to hocket, comprise altogether 3-4 group and draw soft whitewashing operation.
2. according to claim 1 a kind of without chrome tanning pigskin head layer upper leather preparation technology, it is characterized in that: in described main tanning step, before adding described tanning agent, first add sodium formiate, sodium bicarbonate and phospho-glycerol three ester, stir 60-70min, the amount adding described aluminum tanning agent is successively 2.0-2.2%, described glutaraldehyde tanning agent is 6.0-6.5%, the amount of described glutaraldehyde tanning agent evenly divides three parts, successively add respectively for three times, and constantly stir, add other compositions of becoming owner of in tanning afterwards again, add sodium formiate successively, antioxidant, tannin, iron powder, mould inhibitor and sodium bicarbonate, the scope of the amount of described main tanning ancillary component is 8.0-12.0%, finally stir 300-500min.
3. according to claim 2 a kind of without chrome tanning pigskin head layer upper leather preparation technology, it is characterized in that: described mould inhibitor comprises TCMTB(2-thiocyanogen methyl sulfuration benzothiazole) and OIT(octylisothiazolinone), the mass ratio of described TCMTB and described OIT consumption is 1:1-1:2.
4. according to claim 2 a kind of without chrome tanning pigskin head layer upper leather preparation technology, it is characterized in that: the amount that described second time sodium bicarbonate adds is 1.5-2.0%, be divided into five times and add, every minor tick 30-35min.
5. according to claim 1 a kind of without chrome tanning pigskin head layer upper leather preparation technology, it is characterized in that: carry out drum after described main tanning step successively and take horse and leave standstill, setting-out, get rid of soft and shaving deburring step, the bilayer thickness controlling described leather in described shaving step is 2.0-2.4mm.
6. according to claim 1 a kind of without chrome tanning pigskin head layer upper leather preparation technology, it is characterized in that: the composite tanning agent adopted in described retanning step comprises acrylate resin tanning agent, the Caesalpinia spinosaKuntze vegetable tanning agent of improvement and glutaraldehyde tanning agent, the amount that described acrylate resin tanning agent adds is 2.0-2.5%, the amount that the Caesalpinia spinosaKuntze vegetable tanning agent of described improvement adds is 2.2-2.5%, add rear stirring 90-100min, add retanning ancillary component afterwards, then stir 250-300min.
7. according to claim 6 a kind of without chrome tanning pigskin head layer upper leather preparation technology, it is characterized in that: described retanning ancillary component comprises toughner, surfactivity defrosting compound and retanning filler, finally adding sodium bicarbonate regulates pH to be 4.2-4.3, and the amount that described retanning ancillary component adds is 6.0-8.5%.
8. according to claim 1 a kind of without chrome tanning pigskin head layer upper leather preparation technology, it is characterized in that: add the vulcanization accelerator for improving leather machine performance in described water squeezing neutralization procedure, the amount added is 1.0-1.2%.
9. according to claim 1 a kind of without chrome tanning pigskin head layer upper leather preparation technology, it is characterized in that: described dyeing and fat-liquoring step is divided into dyeing process and stuffing operation, dyestuff, diffusant, migration inhibitor and surface active agent is added in described dyeing process, the total amount that described diffusant, migration inhibitor and surface active agent add is 7.0-9.5%, the fatting agent added in described stuffing operation comprises sulfonation synthetic oil and sulfited fish oil, the total amount added is 6.0-8.0%, finally regulates pH and stirs.
10. according to claim 9 a kind of without chrome tanning pigskin head layer upper leather preparation technology, it is characterized in that: described in described dyeing and fat-liquoring step, dyeing process and stuffing operation add the formic acid of 1.5-1.8% as neutralizing agent after all completing, adjustment pH is 3.9-4.0, finally stir, churning time is 100-120min.
CN201610050180.3A 2016-01-26 2016-01-26 One kind is without chrome tanning pigskin head layer upper leather preparation technology Active CN105506196B (en)