CN105112809A - 一种球磨机用高碳低铬耐磨钢球及其制备方法 - Google Patents

一种球磨机用高碳低铬耐磨钢球及其制备方法 Download PDF

Info

Publication number
CN105112809A
CN105112809A CN201510485164.2A CN201510485164A CN105112809A CN 105112809 A CN105112809 A CN 105112809A CN 201510485164 A CN201510485164 A CN 201510485164A CN 105112809 A CN105112809 A CN 105112809A
Authority
CN
China
Prior art keywords
steel ball
insulation
ball
stove
ball mill
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201510485164.2A
Other languages
English (en)
Inventor
周浩
周洁
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Huoqiu Zhongzhen Wear-Resistant Material Co Ltd
Original Assignee
Huoqiu Zhongzhen Wear-Resistant Material Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Huoqiu Zhongzhen Wear-Resistant Material Co Ltd filed Critical Huoqiu Zhongzhen Wear-Resistant Material Co Ltd
Priority to CN201510485164.2A priority Critical patent/CN105112809A/zh
Publication of CN105112809A publication Critical patent/CN105112809A/zh
Pending legal-status Critical Current

Abstract

本发明公开了一种球磨机用高碳低铬耐磨钢球及其制备方法,其各化学成分及质量百分比为:C0.3-0.6、Si1.6-2.2、Mn0.5-0.9、Cr0.2-0.4、Ni0.15-0.25、Cu0.1-0.2、B0.4-0.8、W0.3-0.6、Al0.1-0.2、Zr0.2-0.3、Er0.05-0.07、Yb0.04-0.06、S≤0.04、P≤0.04、余量为Fe。本发明制得的钢球具有硬度高、耐磨性好,磨耗低,韧性好,破碎少的优点,可明显提高球磨机运转率,降低生产成本,具有很好的经济效益。

Description

一种球磨机用高碳低铬耐磨钢球及其制备方法
技术领域
本发明涉及铸铁材料技术领域,具体涉及一种球磨机用高碳低铬耐磨钢球及其制备方法。
背景技术
球磨机钢球是球磨机设备研磨物料介质,通过球磨机钢球之间钢球与物料之间的碰撞摩擦产生磨剥作用,重要的基础零部件,尤其是精密工业钢球在国民经济发展中起着巨大作用,广泛应用于水泥建材、金属矿山、煤浆火电、化学工程、陶瓷等行业的粉体制备与超细深加工。钢球是球磨机主要的易磨损件,其工作繁重,工作条件苛刻,因此对钢球材质的耐磨性和韧性具有较高的要求。
发明内容
本发明的目的在于针对现有技术的不足,提供一种球磨机用高碳低铬耐磨钢球及其制备方法。
为实现上述目的,本发明采用的技术方案如下:
一种球磨机用高碳低铬耐磨钢球,其各化学成分及质量百分比为:C1.3-1.6、Si1.6-2.2、Mn0.5-0.9、Cr0.2-0.4、Ni0.15-0.25、Cu0.1-0.2、B0.4-0.8、W0.3-0.6、Al0.1-0.2、Zr0.2-0.3、Er0.05-0.07、Yb0.04-0.06、S≤0.04、P≤0.04、余量为Fe。
一种球磨机用高碳低铬耐磨钢球的制备方法,包括以下步骤:
(1)在中频感应炉中进行熔炼,先加入废钢、生铁、废旧石墨电极、硅铁熔清,再依次加入硼铁、锰铁、铬铁、铜、镍,待其全部熔化后调整铁水成分,在出炉前5-8min内先后加入钨铁和锆铁,在出炉前4-6min内加入纯铝进行脱氧,出炉前进行化学成分分析,合格后即可出炉,铁水出炉温度控制在1525-1565℃;
(2)在包内冲入稀土硅铁合金变质剂进行变质孕育处理,变质剂使用前进行200-250℃的预热,变质孕育处理温度为1500-1530℃,然后往包内撒入适量的珍珠岩保温聚渣覆盖剂覆盖,并镇静5-10min,扒渣后进行浇注,浇注温度控制在1480-1510℃;
(3)将上述得到的高锰钢进行热处理:先加热至480-560℃,保温3-6h,再加热至850-900℃,保温2-4h,雾冷淬火后再在200-250℃下回火4-7h,然后加热至680-740℃,保温3-5h,再加热至1025-1060℃,保温3-4h,油冷淬火后再在280-360℃下回火6-8h,空冷至室温即可。
本发明的有益效果:
(1)本发明成分设计合理,通过调整C、Cr的含量以及添加适量的Ni、B、W、Zr等元素,可以起到很好的固溶强化、细晶强化作用,同时可以形成细小而弥散分布的硬质颗粒,也可以抑制奥氏体基体向珠光体的转变,促进马氏体基体的形成,提高了钢球的韧性和硬度;
(2)本发明热处理工艺合理,经过两次淬火以及相应的回火处理后,奥氏体变为马氏体,组织细化且均匀致密,增强钢球的耐磨性、韧性和抗冲击能力;
(3)本发明制得的钢球具有硬度高、耐磨性好,磨耗低,韧性好,破碎少的优点,可明显提高球磨机运转率,降低生产成本,具有很好的经济效益。
具体实施方式
一种球磨机用高碳低铬耐磨钢球,其各化学成分及质量百分比为:C1.3-1.6、Si1.6-2.2、Mn0.5-0.9、Cr0.2-0.4、Ni0.15-0.25、Cu0.1-0.2、B0.4-0.8、W0.3-0.6、Al0.1-0.2、Zr0.2-0.3、Er0.05-0.07、Yb0.04-0.06、S≤0.04、P≤0.04、余量为Fe。
一种球磨机用高碳低铬耐磨钢球的制备方法,包括以下步骤:
(1)在中频感应炉中进行熔炼,先加入废钢、生铁、废旧石墨电极、硅铁熔清,再依次加入硼铁、锰铁、铬铁、铜、镍,待其全部熔化后调整铁水成分,在出炉前5-8min内先后加入钨铁和锆铁,在出炉前4-6min内加入纯铝进行脱氧,出炉前进行化学成分分析,合格后即可出炉,铁水出炉温度控制在1525-1565℃;
(2)在包内冲入稀土硅铁合金变质剂进行变质孕育处理,变质剂使用前进行200-250℃的预热,变质孕育处理温度为1500-1530℃,然后往包内撒入适量的珍珠岩保温聚渣覆盖剂覆盖,并镇静5-10min,扒渣后进行浇注,浇注温度控制在1480-1510℃;
(3)将上述得到的高锰钢进行热处理:先加热至480-560℃,保温3-6h,再加热至850-900℃,保温2-4h,雾冷淬火后再在200-250℃下回火4-7h,然后加热至680-740℃,保温3-5h,再加热至1025-1060℃,保温3-4h,油冷淬火后再在280-360℃下回火6-8h,空冷至室温即可。
经检验,产品化学成分为C1.45%、Si1.96%、Mn0.74%、Cr0.31%、Ni0.19%、Cu0.11%、B0.53%、W0.47%、Al0.13%、Zr0.28%、Er0.062%、Yb0.055%、S0.032%、P0.026%、余量为Fe。力学性能为:硬度:64.5HRC,冲击韧性:24.7J/cm2

Claims (2)

1.一种球磨机用高碳低铬耐磨钢球,其特征在于,其各化学成分及质量百分比为:C1.3-1.6、Si1.6-2.2、Mn0.5-0.9、Cr0.2-0.4、Ni0.15-0.25、Cu0.1-0.2、B0.4-0.8、W0.3-0.6、Al0.1-0.2、Zr0.2-0.3、Er0.05-0.07、Yb0.04-0.06、S≤0.04、P≤0.04、余量为Fe。
2.一种如权利要求1所述的球磨机用高碳低铬耐磨钢球的制备方法,其特征在于包括以下步骤:
(1)在中频感应炉中进行熔炼,先加入废钢、生铁、废旧石墨电极、硅铁熔清,再依次加入硼铁、锰铁、铬铁、铜、镍,待其全部熔化后调整铁水成分,在出炉前5-8min内先后加入钨铁和锆铁,在出炉前4-6min内加入纯铝进行脱氧,出炉前进行化学成分分析,合格后即可出炉,铁水出炉温度控制在1525-1565℃;
(2)在包内冲入稀土硅铁合金变质剂进行变质孕育处理,变质剂使用前进行200-250℃的预热,变质孕育处理温度为1500-1530℃,然后往包内撒入适量的珍珠岩保温聚渣覆盖剂覆盖,并镇静5-10min,扒渣后进行浇注,浇注温度控制在1480-1510℃;
(3)将上述得到的高锰钢进行热处理:先加热至480-560℃,保温3-6h,再加热至850-900℃,保温2-4h,雾冷淬火后再在200-250℃下回火4-7h,然后加热至680-740℃,保温3-5h,再加热至1025-1060℃,保温3-4h,油冷淬火后再在280-360℃下回火6-8h,空冷至室温即可。
CN201510485164.2A 2015-08-10 2015-08-10 一种球磨机用高碳低铬耐磨钢球及其制备方法 Pending CN105112809A (zh)