CN104878538A - 一种具有吸湿防水功能的针织面料及其制备方法 - Google Patents

一种具有吸湿防水功能的针织面料及其制备方法 Download PDF

Info

Publication number
CN104878538A
CN104878538A CN201510287622.1A CN201510287622A CN104878538A CN 104878538 A CN104878538 A CN 104878538A CN 201510287622 A CN201510287622 A CN 201510287622A CN 104878538 A CN104878538 A CN 104878538A
Authority
CN
China
Prior art keywords
moisture absorption
preparation
water
knit fabric
proof
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201510287622.1A
Other languages
English (en)
Inventor
颜峰
许畅
单苗苗
林立虎
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shanghai Challenge Textile Co Ltd
Original Assignee
Shanghai Challenge Textile Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shanghai Challenge Textile Co Ltd filed Critical Shanghai Challenge Textile Co Ltd
Priority to CN201510287622.1A priority Critical patent/CN104878538A/zh
Publication of CN104878538A publication Critical patent/CN104878538A/zh
Pending legal-status Critical Current

Abstract

本发明涉及一种具有吸湿防水功能的针织面料及其制备方法,针织面料正面具有防水功能,反面具有亲水功能。制备方法包括:将针织面料预缩、预定型、染色、亲水整理、正面防水整理、验布打卷,即可。本发明面料具有良好的吸湿防水功能,制备工艺简单,成本低,具有良好的应用前景。

Description

一种具有吸湿防水功能的针织面料及其制备方法
技术领域
本发明属于针织面料领域,特别涉及一种具有吸湿防水功能的针织面料及其制备方法。
背景技术
随着人们生活水平的不断提高,大家对服装的要求也越来越高。人们已经不再仅仅满足于对服装款式、颜色等方面的要求,功能性的服装也渐渐成为一种流行趋势。
目前的纺织品加工中,有的是在纤维中直接添加助剂形成功能化,有的是通过整理技术形成功能化;而且,单一功能的产品比较多,因此开发多功能性的面料也已经成为市场的发展方向之一。
发明内容
本发明所要解决的技术问题是提供一种具有吸湿防水功能的针织面料及其制备方法,该面料具有良好的吸湿防水功能,制备工艺简单,成本低,具有良好的应用前景。
本发明的一种具有吸湿防水功能的针织面料,所述针织面料正面具有防水功能,反面具有亲水功能。
本发明的一种具有吸湿防水功能的针织面料的制备方法,包括:
将针织面料预缩、预定型、染色、反面亲水整理、正面防水整理、验布打卷,即可;其中,亲水整理具体包括:(1)采用浸渍法在染浴中做亲水整理,亲水助剂用量为2~4%(o.w.f),处理温度为40℃,处理时间为20~30min;(2)脱水;(3)烘干;
防水整理具体包括:(1)采用防水整理液进行泡沫整理,织物的带液率为15%~30%;(2)预烘;(3)焙烘。
所述预缩工艺的具体参数为:去油剂:1~2g/L;温度:70~90℃;时间:10~20min。
所述预定型工艺的具体参数为:温度:180~200℃;车速20~30m/min。
所述染色工艺的具体参数为:温度:130~135℃;时间:20~30min。
所述亲水助剂包括亲水整理剂和pH调节剂。
所述烘干工艺的具体参数为:温度:110~130℃;车速20~30m/min。
所述防水整理液的组成为:防水整理剂4~8%、发泡剂0.2~0.4%、pH调节剂0.5~0.6%。
所述预烘温度为120~140℃,预烘时间为30~40s。
所述焙烘温度为140~160℃,焙烘时间为60~70s。
有益效果
本发明制备工艺简单,成本较低,具有良好的应用前景;制备的面料功能新颖,较好地满足人们对多功能面料的需求,具有良好的开发前景。
附图说明
图1为本发明的整理工艺流程图。
具体实施方式
下面结合具体实施例,进一步阐述本发明。应理解,这些实施例仅用于说明本发明而不用于限制本发明的范围。此外应理解,在阅读了本发明讲授的内容之后,本领域技术人员可以对本发明作各种改动或修改,这些等价形式同样落于本申请所附权利要求书所限定的范围。
实施例1
面料种类:DTY螺纹针织面料;
预缩过程:去油剂:1.5g/L;温度:80℃;时间:15min;
预定型过程:温度:180℃,车速20m/min;
染色过程:染色温度:132℃,时间:30min;
反面亲水整理:(1)浸渍法亲水处理,亲水整理液为亲水整理剂(o.w.f)2%、pH调节剂;温度40℃,时间为20min;(2)脱水;(3)烘干,温度为130℃,车速为20m/min;
正面防水整理:(1)防水整理液泡沫整理,防水整理液包括防水整理剂6%、发泡剂0.2%、pH调节剂0.5%,使用泡沫整理机将上述防水整理剂涂覆在织物的正面,织物的带液率约为25%;(2)预烘,温度为130℃,时间约为20s;(3)焙烘,温度为160℃,时间约为60s。
效果测试:
实施例2
面料种类:DTY汗布针织面料;
预缩过程:去油剂:2g/L,纯碱:1g/L;温度:95℃;时间:20min;
预定型过程:温度:180℃,车速20m/min;
染色过程:染色温度:132℃,时间:30min;
反面亲水整理:(1)浸渍法亲水处理,亲水整理液为亲水整理剂(o.w.f)3%、pH调节剂;温度40℃,时间为20min;(2)脱水;(3)烘干,温度为130℃,车速为20m/min;
正面防水整理:(1)防水整理液泡沫整理,防水整理液包括防水整理剂6%、发泡剂0.2%、pH调节剂0.5%,使用泡沫整理机将上述防水整理剂涂覆在织物的正面,织物的带液率约为30%;(2)预烘,温度为130℃,时间约为20s;(3)焙烘,温度为160℃,时间约为40s。
效果测试:

Claims (10)

1.一种具有吸湿防水功能的针织面料,其特征在于:所述针织面料正面具有防水功能,反面具有亲水功能。
2.一种具有吸湿防水功能的针织面料的制备方法,包括:
将针织面料预缩、预定型、染色、反面亲水整理、正面防水整理、验布打卷,即可;其中,亲水整理具体包括:(1)采用浸渍法在染浴中做亲水整理,亲水助剂用量为2~4%(o.w.f),处理温度为40℃,处理时间为20~30min;(2)脱水;(3)烘干;
防水整理具体包括:(1)采用防水整理液进行泡沫整理,织物的带液率为15%~30%;(2)预烘;(3)焙烘。
3.根据权利要求2所述的一种具有吸湿防水功能的针织面料的制备方法,其特征在于:所述预缩工艺的具体参数为:去油剂:1~2g/L;温度:70~90℃;时间:10~20min。
4.根据权利要求2所述的一种具有吸湿防水功能的针织面料的制备方法,其特征在于:所述预定型工艺的具体参数为:温度:180~200℃;车速20~30m/min。
5.根据权利要求2所述的一种具有吸湿防水功能的针织面料的制备方法,其特征在于:所述染色工艺的具体参数为:温度:130~135℃;时间:20~30min。
6.根据权利要求2所述的一种具有吸湿防水功能的针织面料的制备方法,其特征在于:所述亲水助剂包括亲水整理剂和pH调节剂。
7.根据权利要求2所述的一种具有吸湿防水功能的针织面料的制备方法,其特征在于:所述烘干工艺的具体参数为:温度:110~130℃;车速20~30m/min。
8.根据权利要求2所述的一种具有吸湿防水功能的针织面料的制备方法,其特征在于:所述防水整理液的组成为:防水整理剂4~8%、发泡剂0.2~0.4%、pH调节剂0.5~0.6%。
9.根据权利要求2所述的一种具有吸湿防水功能的针织面料的制备方法,其特征在于:所述预烘温度为120~140℃,预烘时间为30~40s。
10.根据权利要求2所述的一种具有吸湿防水功能的针织面料的制备方法,其特征在于:所述焙烘温度为140~160℃,焙烘时间为60~70s。
CN201510287622.1A 2015-05-29 2015-05-29 一种具有吸湿防水功能的针织面料及其制备方法 Pending CN104878538A (zh)