CN104817802A - 一种高抓地力橡胶鞋底及其制备方法 - Google Patents

一种高抓地力橡胶鞋底及其制备方法 Download PDF

Info

Publication number
CN104817802A
CN104817802A CN201510166165.0A CN201510166165A CN104817802A CN 104817802 A CN104817802 A CN 104817802A CN 201510166165 A CN201510166165 A CN 201510166165A CN 104817802 A CN104817802 A CN 104817802A
Authority
CN
China
Prior art keywords
parts
rubber
high grip
sulphur
poly
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201510166165.0A
Other languages
English (en)
Other versions
CN104817802B (zh
Inventor
卢鑫
丁思博
罗显发
廖毅彬
郭彩莲
周小兰
林荷香
林江
金校红
郑荣大
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Maotai Fujian New Material Technology Co ltd
Original Assignee
Maotai Fujian Shoes Material Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Maotai Fujian Shoes Material Co Ltd filed Critical Maotai Fujian Shoes Material Co Ltd
Priority to CN201510166165.0A priority Critical patent/CN104817802B/zh
Publication of CN104817802A publication Critical patent/CN104817802A/zh
Application granted granted Critical
Publication of CN104817802B publication Critical patent/CN104817802B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种鞋底,提供一种具有高抓地力的橡胶鞋底及其制备方法,所述高抓地力橡胶鞋底的组成包括天然橡胶、聚降冰片烯橡胶、溴化丁基橡胶、矿物油、白炭黑、防老剂、聚乙二醇、硅烷偶联剂、聚乙烯蜡、氧化锌、硫磺、硫化促进剂,将以上组分材料除硫磺、硫化促进剂以外的胶料放入密炼机中密炼,115-120度排胶,室温放置24小时,然后在双辊开炼机上混炼,并加入准确称量的硫磺、硫化促进剂,混炼均匀后,以均匀片状出片,最后将物料裁成鞋底形状放入橡胶鞋模中硫化成型,即得到高抓地力橡胶鞋底。

Description

一种高抓地力橡胶鞋底及其制备方法
技术领域
本发明属于有机高分子化合物技术领域,特别涉及一种高抓地力橡胶鞋底及其制备方法。
背景技术
聚降冰片烯橡胶,保留着双环结构,每两个相邻碳原子之间都相互固定,结构单元中的碳原子活动困难,因此具有较高的玻璃化转变温度和热分解温度。聚降冰片烯橡胶的分子结构是若干链段依靠化学键链接起来的大分子,大分子链之间相互缠结,支链的存在加剧了相互缠结。在周期性外力作用下产生一定的形变,由于分子链之间缠结使得高聚物在拉伸-回缩循环需要克服一部分分子链之间的摩擦阻力,这种形变落后于应力的过程中,将机械能转化成热能的形式耗散掉,进一步体现为具有高的摩擦系数,即高抓地力。
发明内容
本发明的目的在于提供一种具有抓地力好、机械强度高等特点的高抓地力橡胶鞋底,以及制备前述高抓地力橡胶鞋底的制备方法。
为实现上述目的,本发明采用如下技术方案:一种高抓地力橡胶鞋底,由组分材料由天然橡胶、聚降冰片烯橡胶、溴化丁基橡胶、白炭黑、矿物油、氧化锌、防老剂、聚乙二醇、硅烷偶联剂、聚乙烯蜡、硫磺、硫化促进剂制备而成。
其中:所述一种高抓地力橡胶鞋底的各组分材料按重量份表示为:
天然橡胶                           15 份
聚降冰片烯橡胶                     40 - 55 份
溴化丁基橡胶                       8 -15 份
白炭黑                             25 - 35 份
矿物油                             25 - 35 份
氧化锌                             1 - 3 份
防老剂                             1 - 2 份
聚乙二醇                           2 - 4 份
硅烷偶联剂                         2 - 3 份
聚乙烯蜡                           2 - 3 份
硫磺                               2 - 3 份
硫化促进剂                         2 - 3 份。
进一步的,各组分材料的重量份优选为:
天然橡胶                           15 份
聚降冰片烯橡胶                     50 份
溴化丁基橡胶                       10 份
白炭黑                             30 份
矿物油                             30 份
氧化锌                             1份
防老剂                             1.5 份
聚乙二醇                           3 份
硅烷偶联剂                         3 份
聚乙烯蜡                           2 份
硫磺                               2 份
硫化促进剂                         2.2 份。
其中, 所述聚降冰片烯橡胶是分子量在200万-500万道尔顿的聚降冰片烯橡胶。
其中, 所述溴化丁基橡胶的含溴量大于1.5%。
一种制备前述高抓地力橡胶鞋底的制备方法,按照配方比例称量天然橡胶、聚降冰片烯橡胶、溴化丁基橡胶、白炭黑、矿物油、氧化锌、防老剂、聚乙二醇、硅烷偶联剂、聚乙烯蜡、硫磺、硫化促进剂,将组分材料除硫磺、硫化促进剂以外的胶料放入密炼机中密炼,110-120度排胶,室温放置24小时,然后在双辊开炼机上混炼,并加入准确称量的硫磺、硫化促进剂,混炼均匀后,以均匀片状出片,最后将物料裁成鞋底形状放入橡胶鞋模中硫化成型,即得到高抓地力橡胶鞋底。
通过采取前述技术方案,本发明具有如下有益效果:
1,本发明高抓地力橡胶鞋底的效果显著,具体体现在鞋底防滑性能优越,干式、湿式的止滑系数分别高达1.17、0.70,明显优于现有技术的防滑鞋底。这是因为聚降冰片烯橡胶结构中反式基的分布形成了分子间运动的高阻抗力,具有高的摩擦系数。
2. 本发明高阻尼发泡材料的主体材料是聚降冰片烯橡胶,具有表面多孔性、极强吸附力、与碳氢化合物具有高度亲和性等特点,可添加大量的填充油而不影响其他物性,提高了加工操作性能,并降低生产成本。
具体实施方式
现结合具体实施例对本发明进一步说明。
实施例1:
本实施例中, 一种高抓地力橡胶鞋底由以下组分按重量份组成:
天然橡胶                           15 份
聚降冰片烯橡胶                     50 份
溴化丁基橡胶                       10 份
白炭黑                             30 份
矿物油                             30 份
氧化锌                             1份
防老剂1010                         1.5 份
聚乙二醇                           3 份
硅烷偶联剂Si69                     3 份
聚乙烯蜡                           2 份
硫磺                               2 份
硫化促进剂                         2.2 份。
将组分材料除硫磺、硫化促进剂以外的胶料放入密炼机中密炼,119度排胶,室温放置24小时,然后在双辊开炼机上混炼,并加入准确称量的硫磺、硫化促进剂,混炼均匀后,以均匀片状出片,最后将物料裁成鞋底形状放入橡胶鞋模中硫化成型,即得到高抓地力橡胶鞋底。
上述制备得到的一种高抓地力橡胶鞋底,密度1.08g/cm3,硬度A 62,DIN耐磨143 mm3,拉伸强度18.2MPa,撕裂强度75N/mm,止滑系数干式后跟1.04前掌1.01平滑1.17,止滑系数湿式后跟0.66前掌0.66平滑0.70,止滑系数湿冰面平滑0.30。
实施例2:
本实施例中, 一种高抓地力橡胶鞋底的制备方法基本与实施例1中的制备方法相同,所不同的是:
聚降冰片烯橡胶55份、溴化丁基橡胶8份、白炭黑25份、矿物油25份、聚乙二醇2份、硅烷偶联剂2份。
上述制备得到的一种高抓地力橡胶鞋底,密度1.06g/cm3,硬度A 59,DIN耐磨167 mm3,拉伸强度19.3MPa,撕裂强度79N/mm,止滑系数干式后跟1.02前掌1.02平滑1.06,止滑系数湿式后跟0.63前掌0.62平滑0.65,止滑系数湿冰面平滑0.24。
实施例3:
本实施例中, 一种高抓地力橡胶鞋底的制备方法基本与实施例1中的制备方法相同,所不同的是:
聚降冰片烯橡胶45份、溴化丁基橡胶12份、白炭黑35份、矿物油35份、聚乙二醇4份、硅烷偶联剂3份;控制在120度排胶。
上述制备得到的一种高抓地力橡胶鞋底,密度1.16g/cm3,硬度A 69,DIN耐磨231 mm3,拉伸强度15.8MPa,撕裂强度57N/mm,止滑系数干式后跟0.96前掌0.91平滑0.96,止滑系数湿式后跟0.49前掌0.48平滑0.52,止滑系数湿冰面平滑0.16。
实施例4:
本实施例中, 一种高抓地力橡胶鞋底的制备方法基本与实施例1中的制备方法相同,所不同的是:
聚降冰片烯橡胶40份、溴化丁基橡胶15份、白炭黑35份、矿物油25份。
上述制备得到的一种高抓地力橡胶鞋底,密度1.19g/cm3,硬度A 65,DIN耐磨287 mm3,拉伸强度14 MPa,撕裂强度49N/mm,止滑系数干式后跟0.83前掌0.84平滑0.88,止滑系数湿式后跟0.47前掌0.48平滑0.49,止滑系数湿冰面平滑0.11。
将上述实施例1~4的数据整理后,得到如下表1(注:硬度采用GS-706G硬度计测试,DIN耐磨按照GB/T 9867-2008测试,拉伸强度按照GB/T 528-2009 测试,撕裂强度按照GB/T 529-2008测试直角撕裂试片,止滑系数按照TM144:2011测试):
      
表1、实施例1~4制备的高抓地力橡胶鞋底的性能参数对照表
综上所述,按照本发明的高抓地力橡胶鞋底的制备方法制得的高抓地力橡胶鞋底具有抓地力好、机械强度高等特点,特别适合在鞋底等方面应用。
以上所记载,仅为利用本创作技术内容的实施例,任何熟悉本项技艺者运用本创作所做的修饰、变化,皆属本创作主张的专利范围,而不限于实施例所揭示者。

Claims (6)

1.一种高抓地力橡胶鞋底, 其特征在于,由下列原料组成:天然橡胶、聚降冰片烯橡胶、溴化丁基橡胶、白炭黑、矿物油、氧化锌、防老剂、聚乙二醇、硅烷偶联剂、聚乙烯蜡、硫磺、硫化促进剂。
2.根据权利要求1所述高抓地力橡胶鞋底, 其特征在于,各原料的重量份数为:
天然橡胶                           15 份
聚降冰片烯橡胶                     40 - 55 份
溴化丁基橡胶                       8 -15 份
白炭黑                             25 - 35 份
矿物油                             25 - 35 份
氧化锌                             1 - 3 份
防老剂                             1 - 2 份
聚乙二醇                           2 - 4 份
硅烷偶联剂                         2 - 3 份
聚乙烯蜡                           2 - 3 份
硫磺                               2 - 3 份
硫化促进剂                         2 - 3 份。
3. 根据权利要求2所述高抓地力橡胶鞋底,其特征在于,各原料的重量份数为:
天然橡胶                           15 份
聚降冰片烯橡胶                     50 份
溴化丁基橡胶                       10 份
白炭黑                             30 份
矿物油                             30 份
氧化锌                             1份
防老剂                             1.5 份
聚乙二醇                           3 份
硅烷偶联剂                         3 份
聚乙烯蜡                           2 份
硫磺                               2 份
硫化促进剂                         2.2 份。
4. 根据权利要求1或2所述高抓地力橡胶鞋底,其特征在于:聚降冰片烯橡胶是分子量在200万-500万道尔顿的聚降冰片烯橡胶。
5. 根据权利要求1或2所述高抓地力橡胶鞋底,其特征在于:所述溴化丁基橡胶的含溴量大于1.5%。
6. 一种制备权利要求1-5任一所述高抓地力橡胶鞋底的制备方法,其特征在于:先将天然橡胶、聚降冰片烯橡胶、溴化丁基橡胶、白炭黑、矿物油、氧化锌、防老剂、聚乙二醇、硅烷偶联剂、聚乙烯蜡放入密炼机中密炼,115-120度排胶,室温放置24小时,然后在双辊开炼机上混炼,并加入准确称量的硫磺、硫化促进剂,混炼均匀后,以均匀片状出片,最后将物料裁成鞋底形状放入橡胶鞋模中硫化成型,即得到高抓地力橡胶鞋底。
CN201510166165.0A 2015-04-09 2015-04-09 一种高抓地力橡胶鞋底及其制备方法 Active CN104817802B (zh)