CN102134478A - 一种石油钻井用可控膨胀堵漏剂及其生产工艺 - Google Patents

一种石油钻井用可控膨胀堵漏剂及其生产工艺 Download PDF

Info

Publication number
CN102134478A
CN102134478A CN2010101005818A CN201010100581A CN102134478A CN 102134478 A CN102134478 A CN 102134478A CN 2010101005818 A CN2010101005818 A CN 2010101005818A CN 201010100581 A CN201010100581 A CN 201010100581A CN 102134478 A CN102134478 A CN 102134478A
Authority
CN
China
Prior art keywords
lost circulation
petroleum drilling
film forming
spray gun
expandable
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN2010101005818A
Other languages
English (en)
Inventor
唐代绪
何兴贵
刘宝峰
刘振东
侯业贵
宋兆辉
刘从军
高杨
隋旭强
王俊涛
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
China Petrochemical Corp
Drilling Technology Research Institute of Sinopec Shengli Petroleum Administration Bureau
Original Assignee
China Petrochemical Corp
Drilling Technology Research Institute of Sinopec Shengli Petroleum Administration Bureau
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by China Petrochemical Corp, Drilling Technology Research Institute of Sinopec Shengli Petroleum Administration Bureau filed Critical China Petrochemical Corp
Priority to CN2010101005818A priority Critical patent/CN102134478A/zh
Publication of CN102134478A publication Critical patent/CN102134478A/zh
Pending legal-status Critical Current

Abstract

本发明是石油钻井用可控膨胀堵漏剂及其生产工艺,用于对石油勘探开发钻井过程中的漏失进行防漏堵漏。该可控膨胀堵漏剂是一种以膨胀型树脂A和温敏性材料B、成膜材料C为主要原材料的新型堵漏剂,该石油钻井用可控膨胀堵漏剂的生产工艺是,温敏性材料B和成膜材料C在加热的条件下用气动搅拌器配好,喷枪、气管、料管加热到设定温度后,物料经蠕动泵将料送至喷枪,喷枪利用空压机的气压将包衣液雾化,喷到盛有膨胀型树脂A的转动的糖衣锅中,进行喷涂。本发明与现有堵漏剂相比具有原材料来源广泛、产品性能稳定、贮存期较长,适用温度范围广、无毒、堵漏效果好等优点。

Description

一种石油钻井用可控膨胀堵漏剂及其生产工艺
技术领域
本发明石油钻井用可控膨胀堵漏剂及其生产工艺是用于石油勘探开发钻井过程中的漏失进行防漏堵漏的堵漏剂。
背景技术
目前,石油勘探开发在治理井漏的诸多工艺当中,利用各种天然物质加工而成的堵漏材料进行桥塞堵漏是目前较为普遍采用的堵漏方法。长期以来,工程技术人员针对不同情况的井漏,在实践中对各种堵漏材料进行了优选。但是,这些材料的共同缺陷在于:一是堵漏过程中自身的可变形性较差,稍大于漏层孔隙裂缝或是与漏层孔隙裂缝形状不匹配的颗粒就不易进入,在漏层表面形成堆积,并未深入漏层。二是这些堵漏材料不具有膨胀性或只有微小的膨胀量,在外部作用力的作用下不易稳定地滞留在漏层当中。三是大多数堵漏材料加入钻井液后,将影响钻井液的性能。由于上述原因,使用这些材料处理井漏时,往往易造成堵漏效果不佳和堵漏后发生重复性漏失。
为了克服上述缺陷,本发明的目的是研制出一种新型的石油钻井用可控膨胀堵漏剂。
本发明与现有技术相比有以下优点:具有原材料来源广泛、产品性能稳定、贮存期较长,适用温度范围广、无毒、堵漏效果好等优点。实验证明,该可控膨胀堵漏剂具有延迟膨胀性和可变形性,膨胀倍数达100倍以上,抗压强度大于7MPa。
发明内容
本发明是这样实现的,该石油钻井用可控膨胀堵漏剂是一种以膨胀型树脂A和温敏性材料B、成膜材料C为主要原材料的新型堵漏剂,膨胀型树脂A是水溶性树脂类;温敏性材料B是石蜡类材料;成膜材料C是乙烯-乙酸乙烯酯树脂类。C与B的质量配比如下:C∶B=9~10%。由温敏性材料B和成膜材料C组成的包覆材料的利用率为78%。
该石油钻井用可控膨胀堵漏剂的生产工艺是,温敏性材料B和成膜材料C在加热的条件下用气动搅拌器配好,喷枪、气管、料管加热到设定温度后,物料经蠕动泵将料送至喷枪,喷枪利用空压机的气压将包衣液雾化,喷到盛有膨胀型树脂A的转动的糖衣锅中,进行喷涂。
具体实施方式
下面对本发明作详细说明:
本发明选用的膨胀型树脂A(吸水性树脂)原材料来源广泛、性能稳定、环境友好、配制的堵漏剂膨胀倍数高;以温敏性材料B作为可控膨胀堵漏剂的外层材料,原材料来源广泛,在一定的温度条件下能溶解;成膜材料C成膜性好,韧性强,成膜材料C主要是提高膨胀型树脂A外层的包覆材料的成膜性和韧性。
本发明是这样实现的,在喷枪高度为10cm、转速为45rpm、包覆材料(由温敏性材料B和成膜材料C组成)流量为50mL/min、空气流量为60L/min的条件下将温敏性材料B和成膜材料C在加热的条件下用气动搅拌器配好,喷枪、气管、料管加热到包覆材料溶解的温度后,物料经蠕动泵将料送至喷枪,喷枪利用空压机的气压将包衣液雾化,喷到盛有膨胀型树脂A的转动的糖衣锅中,进行喷涂。

Claims (6)

1.一种石油钻井用可控膨胀堵漏剂,其特征在于该石油钻井用可控膨胀堵漏剂是一种以膨胀型树脂A、温敏性材料B和成膜材料C为主要原材料的新型堵漏剂。
2.按权利要求1所述的石油钻井用可控膨胀堵漏剂,其特征在于:膨胀型树脂A是水溶性树脂;温敏性材料B是石蜡材料;成膜材料C是乙烯-乙酸乙烯酯树脂。
3.按权利要求1或2所述的石油钻井用可控膨胀堵漏剂,其特征在于C与B的质量配比如下:C∶B=9~10%。
4.按权利要求1或者2所述的石油钻井用可控膨胀堵漏剂,其特征在于:由温敏性材料B和成膜材料C组成的包覆材料的利用率为78%。
5.按权利要求1或2所述的石油钻井用可控膨胀堵漏剂的生产工艺,其特征在于:温敏性材料B和成膜材料C在加热的条件下用气动搅拌器配好,喷枪、气管、料管加热到设定温度后,物料经蠕动泵将料送至喷枪,喷枪利用空压机的气压将包衣液雾化,喷到盛有膨胀型树脂A的转动的糖衣锅中,进行喷涂。
6.按权利要求5所述的石油钻井用可控膨胀堵漏剂的生产工艺,其特征在于:喷枪高度为10cm、转速为45rpm、包覆材料(温敏性材料B和成膜材料C)流量为50mL/min、空气流量为60L/min。
CN2010101005818A 2010-01-25 2010-01-25 一种石油钻井用可控膨胀堵漏剂及其生产工艺 Pending CN102134478A (zh)