CN100580164C - Method for preparing wool comprising milk protein fiber and wool thereby - Google Patents

Method for preparing wool comprising milk protein fiber and wool thereby Download PDF

Info

Publication number
CN100580164C
CN100580164C CN200510011736A CN200510011736A CN100580164C CN 100580164 C CN100580164 C CN 100580164C CN 200510011736 A CN200510011736 A CN 200510011736A CN 200510011736 A CN200510011736 A CN 200510011736A CN 100580164 C CN100580164 C CN 100580164C
Authority
CN
China
Prior art keywords
minutes
base line
dye
dyeing
acetic acid
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN200510011736A
Other languages
Chinese (zh)
Other versions
CN1865555A (en
Inventor
王启发
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN200510011736A priority Critical patent/CN100580164C/en
Publication of CN1865555A publication Critical patent/CN1865555A/en
Application granted granted Critical
Publication of CN100580164C publication Critical patent/CN100580164C/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a knitting wool preparing method with milk fiber and preparing method, which comprises the following steps: 1. preparing mould line with 20-35 percent milk fiber, one or random combination of 65-80 percent silk, yarn, natural silk, cotton, cashmere; 2. washing line; 3. dyeing; adopting one bathing method, one bathing two-step, two bathing two-step to dye; 4. dewatering; 5. drying. The invention improves milk fiber content with excellent rendition and even dyeing and fastening property, which satisfies the need of people.

Description

Contain the preparation method of knitting wool of milk fibre and the knitting wool of preparation thereof
Technical field
The present invention relates to a kind of preparation method of knitting wool and the knitting wool of preparation thereof, relate in particular to a kind of preparation method of the knitting wool that contains milk fibre and the knitting wool of preparation thereof.
Background technology
Contain 10 kinds of amino acid in the milk fibre, and contain the protein natural moisturizing factor, therefore can play the nutrition skin, make skin soft and moist smooth the human body beneficial.Milk fibre has the gloss as the silk, the soft feel as the cashmere; Also have natural hygroscopicity, lead moistly, wear smooth, comfortable.At present milk fibre is increasing is used to prepare knitting wool jointly with other fiber, the thick cotton spinning apparatus productions of general many employings, and the performance of product can not satisfy the higher requirement of people; In addition, the fastness of the uniformity coefficient of the repeatability of dyeing, dyeing, dyeing is all not ideal enough.
Summary of the invention
The invention provides a kind of preparation method of the knitting wool that contains milk fibre and the knitting wool of preparation thereof.Adopt the knitting wool of the present invention's preparation, its performance can satisfy the higher requirement of people, and the repeatability that has dyeing simultaneously is good, the good advantage of fastness of even dyeing, dyeing, has overcome the deficiency of existing procucts.
Preparation method's the step of knitting wool that the present invention contains milk fibre is as follows:
1, base line
Base line raw material components and percentage by weight consist of:
Milk fibre 20-35%,
One of it silk, wool, silk, cotton, cashmere or be combined as 65-80% arbitrarily,
Base line needed raw material is carried out stripping on spinning equipment, again it is sent into spinning machine and make the base line;
2, wash line
Above-mentioned base line is sent into tape machine to be washed;
3, dyeing
The dyeing of base line after the above-mentioned washing can be adopted one of a, one-bath dyeing, b, one-bath two-step process dyeing, c, two one-bath two-step process dyeings; Its bath raio is 1: 30-40;
(1) use one-bath dyeing, the component of dyestuff and to the percentage by weight of base line (O, W f) are:
1) weak acid dye 0.01-0.1% (O, W, f),
2) the acetic acid pH value of transferring dye liquor to 4-6,
3) levelling agent 0.8-2% (O, W, f),
4) glauber salt 0-10% (O, W, f),
5) acetic acid 1-3% (O, W, f) and softener 2-8% (O, W, mixed liquor f),
One-bath dyeing step: the required above-mentioned base line of having washed is sent into dye vat, add required water by bath raio; Dyeing machine running adds required acetic acid, and every then running adds required levelling agent and glauber salt, weak acid dye successively after 5 minutes, rerunned 30 minutes; Raise 1 ℃ in the every 1-4 of temperature minute in the dye vat then, rise to 85 ℃, raise 1 ℃ in every again 1-3 minute, be raised to 90-100 ℃, insulation running 20-40 minute; Spilling water is cooled to 30-40 ℃, adds the mixed liquor of required acetic acid and softener, and the insulation running is 10-30 minute again, goes out cylinder;
(2) with one-bath two-step process dyeing, the component of dyestuff and to the percentage by weight of base line (O, W f) are:
1) 0.1-0.5% of weak acid dye (O, W, f),
2) 0.05-0.1% of cation dyes (O, W, f),
3) the acetic acid pH value of transferring dye liquor to 5-5.5,
4) glauber salt 0-10% (O, W, f),
5) dispersant 0.3-1.5% (O, W, f),
6) levelling agent 1-3% (O, W, f),
7) acetic acid 1-3% (O, W, f) and softener 3-8% (O, W, mixed liquor f),
One-bath two-step process staining procedure: the required above-mentioned base line of having washed is sent into dye vat, add required water by bath raio; The dyeing machine running adds required acetic acid, turns round to add required glauber salt, dispersant and levelling agent after 5 minutes, reruns 5 minutes, adds weak acid dye, reruns 30 minutes; In the dye vat the every 2-4 of temperature minute then, raise 1 ℃, rise to 50-75 ℃; Add cation dyes, insulation running 5-20 minute; Temperature raise 1 ℃ in every again 2-6 minute in the dye vat then, rose to 90-100 ℃, was incubated 20-50 minute; Spilling water is reduced to 30-40 ℃, adds the mixed liquor of required acetic acid and softener, and the insulation running is 10-30 minute again, goes out cylinder;
(3) use two one-bath two-step process dyeings, first bath when dyeing dye component and to the percentage by weight of base line (O, W, f) or the weight that adds by every premium on currency in the dye vat be:
1) cotton reactive dye 0.5-3% (O, W, f),
2) glauber salt 10-30g/L,
3) soda ash 5-15g/L,
4) anti-be stained with agent 2-6g/L,
5) levelling agent 1-3% (O, W, f),
The first bath staining procedure is sent the required above-mentioned base line of having washed into dye vat, adds required water by bath raio; The dyeing machine running, add the required anti-agent of being stained with, turn round and add required levelling agent after 5 minutes, rerunned 5 minutes, and added required cotton reactive dye, rerun after 10 minutes and to add 1/2 of required glauber salt weight, rerun 1/2 other glauber salt of adding after 10 minutes, rerunned 10 minutes, and added 1/2 of required soda ash weight, rerunned 10 minutes; Raise 1 ℃ in the every 1-4 of temperature minute in the dye vat then, rise to 50-70 ℃, insulation running 5-10 minute adds other 1/2 soda ash, and the insulation running is 20-30 minute again; Spilling water is cooled to 20-40 ℃, emptying then;
The component of second dyestuff when bathing two steps dyeing and to the percentage by weight of base line (O, W f) are:
1) weak acid dye 0.5-1% (O, W, f),
2) cation dyes 0.02-0.05% (O, W, f),
3) acetic acid 1-4% (O, W, f),
4) glauber salt 0-10% (O, W, f),
5) dispersant 0.5-2% (O, W, f),
6) levelling agent 0.5-2% (O, W, f),
7) acetic acid 1-3% (O, W, f) and softener 3-8% (O, W, mixed liquor f),
Second bathes the step of two steps dyeing: add entry again by bath raio in the dye vat of above-mentioned emptying; The dyeing machine running adds required acetic acid, and every running adds required glauber salt, dispersant, levelling agent, weak acid dye successively after 5 minutes, rerunned 30 minutes; Raise 1 ℃ in the every 2-4 of temperature minute in the dye vat then, rise to 50-70 ℃, adds required cation dyes, insulation was turned round 5-20 minute; Temperature raise 1 ℃ in every again 2-4 minute in the dye vat, rose to 90-100 ℃, insulation running 20-60 minute; Spilling water is cooled to 30-40 ℃, adds the mixed liquor of required acetic acid and softener, and insulation running 30 minutes goes out cylinder;
4, dehydration
The above-mentioned base line that dyed look is sent into Water Extraction Machinery, dewatered 10 minutes;
5, oven dry
Base line after the above-mentioned dehydration is sent into dryer, and bake out temperature is 85-95 ℃, dries and obtains knitting wool after 40 minutes.
Use one-bath dyeing in above-mentioned preparation method's step, the component of dyestuff and to the preferred weight percent of base line (O, W f) are:
1) weak acid dye 0.06-0.1% (O, W, f),
2) the acetic acid pH value that transfers to dye liquor to 5.3-6,
3) levelling agent 1.1-2% (O, W, f),
4) glauber salt 5-10% (O, W, f),
5) acetic acid 1-2% (O, W, f) and softener 4-8% (O, W, mixed liquor f);
In above-mentioned preparation method's step with one-bath two-step process dyeing, the component of dyestuff and to the preferred weight percent of base line (O, W f) are:
1) weak acid dye 0.3-0.5% (O, W, f),
2) cation dyes 0.07-0.1% (O, W, f),
3) the acetic acid pH value of transferring dye liquor to 5.2-5.5,
4) glauber salt 4-10% (O, W, f),
5) dispersant 0.6-1.5% (O, W, f),
6) levelling agent 1-1.5% (O, W, f),
7) (O, W is f) with softener 5-8% (O, W, mixed liquor f) for acetic acid 1-2%.
Use two one-bath two-step process dyeings in above-mentioned preparation method's step, first bath when dyeing dye component and to the preferred weight percent of base line (O, W, f) or the preferred weight that adds by every premium on currency in the dye vat be:
1) cotton reactive dye 0.8-3% (O, W, f),
2) glauber salt 16-30g/L,
3) soda ash 10-15g/L,
4) anti-be stained with agent 4-6g/L,
5) levelling agent 2-3% (O, W, f).
Bathe the dyeing of two steps with two in above-mentioned preparation method's step, the component of second dyestuff when bathing two steps dyeing and to the preferred weight percent of base line (O, W f) are:
1) weak acid dye 0.7-1% (O, W, f),
2) cation dyes 0.03-0.05% (O, W, f),
3) acetic acid 2-4% (O, W, f),
4) glauber salt 4-10% (O, W, f),
5) dispersant 1.1-2% (O, W, f),
6) levelling agent 1-2% (O, W, f),
7) (O, W is f) with softener 5-8% (O, W, mixed liquor f) for acetic acid 1-2%.
The content of milk fibre is than higher in the raw material of base line of the present invention, and therefore to have advantage, the performance of milk fibre more outstanding for prepared knitting wool, more is received by the market.
Base line of the present invention adopts spinning equipment, and institute's base line is even, smooth, phozy, can reach the requirement of elaboration.
The one-bath dyeing that the present invention adopts be at dyeing such as the azelon in the knitting wool such as the azelon in the milk fibre, wool, cashmere, silks, and other fiber is not painted, can obtain the sensation that snow flakes are whirling.This colouring method is simple, be convenient to operation, and dyeing reproducibility is good, dyefastness is good, is more suitable for dying shallow, middle light color.
The one-bath two-step process dyeing that the present invention adopts be the dyeing at azelon in the knitting wool and the polyethylene nitrile two types of fibers in the milk fibre, thereby two kinds of fibers that milk fibre is comprised is all caught look, knitting wool bright-colored, color is full.
Two one-bath two-step process dyeings that the present invention adopts are at fine cellulose fiber, as cotton, day silk; Protein fibre; The polyethylene nitrile stock-dye, or obtain effect homochromy or the folder flower, be fit to dye dark color.
The specific embodiment
Adopt the step of above-mentioned three kinds of colouring methods and condition control dyeing, dye that the colorrendering quality of knitting wool is good, dyefastness is good, color is even, bright-coloured, color is wide in variety, can satisfy the demand in market.
Raw material required for the present invention, equipment all can be bought on market.
Embodiment 1
1, base line
40 kilograms of milk fibres, day 80 kilograms of silks, wool are mixed for 80 kilograms, on spinning equipment, make bar, again it is sent into spinning machine and make the base line;
2, wash line
Above-mentioned base line is sent into GM372 molded lines belt four groove tape machines to be washed;
3, dyeing
The above-mentioned base line of having washed is put into dye vat for 100 kilograms, add 3000 kg of water; The dyeing machine running, it is 4 that adding acetic acid makes the dye liquor pH value, every then running added 0.8 kilogram of levelling agent, 0.01 kilogram of red 10B in pula in 5 minutes successively, rerunned 30 minutes; Temperature raise 1 ℃ in per 1 minute in the dye vat then, rose to 85 ℃, raise 1 ℃ in per again 1 minute, rose to 90 ℃, insulation running 20 minutes; Spilling water is reduced to 30 ℃, adds 1 kilogram of acetic acid and 2 kilograms of softener mixed liquors, and the insulation running is 10 minutes again, goes out cylinder;
4, dehydration
The above-mentioned base line that dyed look is sent into Z751-1200 type centrifugal type Water Extraction Machinery, dewatered 10 minutes;
5, oven dry
Base line after the above-mentioned dehydration is sent into K031 type hot air type reeled yarn drying machine, and bake out temperature is 85 ℃, and drying time 40 minutes obtains knitting wool.
Embodiment 2
1, base line
50 kilograms of milk fibres, 60 kilograms of silks, cashmere are mixed for 90 kilograms, on spinning equipment, make bar, again it is sent into spinning machine and make the base line;
2, wash line
Above-mentioned base line is sent into GM372 molded lines belt four groove tape machines to be washed;
3, dyeing
The above-mentioned base line of having washed is put into dye vat for 100 kilograms, add 3700 kg of water; Dyeing machine running, adding acetic acid, to make the dye liquor pH value be 5.3, every then running added 1.1 kilograms of levelling agents and 5 kilograms of glauber salt, 0.027 kilogram of polar yellow GN in 5 minutes successively 100%, the red B in 0.033 pula, rerunned 30 minutes; Temperature raise 1 ℃ in per 3 minutes in the dye vat then, rose to 85 ℃, raise 1 ℃ in per again 2 minutes, rose to 98 ℃, insulation running 30 minutes; Spilling water is reduced to 35 ℃, adds 2 kilograms of acetic acid and 4 kilograms of softener mixed liquors, and the insulation running is 20 minutes again, goes out cylinder; ,
4, dehydration
The above-mentioned base line that dyed look is sent into Z751-1200 type centrifugal type Water Extraction Machinery, dewatered 10 minutes;
5, oven dry
Base line after the above-mentioned dehydration is sent into K031 type hot air type reeled yarn drying machine, and bake out temperature is 90 ℃, and drying time 40 minutes obtains knitting wool.
Embodiment 3
1, base line
50 kilograms of milk fibres, cotton 20 kilograms, 130 kilograms wools are mixed, on spinning equipment, make bar, again it is sent into spinning machine and make the base line;
2, wash line
Above-mentioned base line is sent into GM372 molded lines belt four groove tape machines to be washed;
3, dyeing
The above-mentioned base line of having washed is put into dye vat for 100 kilograms, add 4000 kg of water; Dyeing machine running, adding acetic acid, to make the dye liquor pH value be 6, every then running added 2 kilograms of levelling agents and 10 kilograms of glauber salt, 0.067 kilogram of this bright blue 5GMA of pleasure, 0.033 kilogram of this blue 2RLA of pleasure in 5 minutes successively, rerunned 30 minutes; Temperature raise 1 ℃ in per 4 minutes in the dye vat then, rose to 85 ℃, raise 1 ℃ in per again 3 minutes, rose to 100 ℃, insulation running 40 minutes; Spilling water is reduced to 40 ℃, adds 3 kilograms of acetic acid and 8 kilograms of softener mixed liquors, and the insulation running is 30 minutes again, goes out cylinder;
4, dehydration
The above-mentioned base line that dyed look is sent into Z751-1200 type centrifugal type Water Extraction Machinery, dewatered 10 minutes;
5, oven dry
Base line after the above-mentioned dehydration is sent into K031 type hot air type reeled yarn drying machine, and bake out temperature is 95 ℃, and drying time 40 minutes obtains knitting wool.
Embodiment 4
1, base line
40 kilograms of milk fibres, 80 kilograms of sky silks, 40 kilograms of cashmere, 40 kilograms of wools are mixed, on spinning equipment, make bar, again it is sent into spinning machine and make the base line;
2, wash line
Above-mentioned base line is sent into GM372 molded lines belt four groove tape machines to be washed;
3, dyeing
The above-mentioned base line of having washed is sent into dye vat for 100 kilograms, add 3000 kg of water; The dyeing machine running adds acetic acid, and making the dye liquor pH value is 5, turns round to add 0.3 kilogram of dispersant and 1 kilogram of levelling agent after 5 minutes, reruns to add 0.09 kilogram of red B in pula, 0.01 kilogram of red 10B in pula after 5 minutes, reruns 30 minutes; Temperature raise 1 ℃ in per 2 minutes in the dye vat then, rose to 50 ℃; Add 0.04 kilogram of cationic red GRL, the grand pake purpke 3BLH of 0.01 kilogram calorie magnetic, insulation running 5 minutes; Temperature raise 1 ℃ to 90 ℃ in per 2 minutes in the dye vat then, insulation running 20 minutes; Spilling water is cooled to 30 ℃, adds 1 kilogram of acetic acid and 3 kilograms of softener mixed liquors, and the insulation running is 10 minutes again, goes out cylinder;
4, dehydration
The above-mentioned base line that dyed look is sent into Z751-1200 type centrifugal type Water Extraction Machinery, dewatered 10 minutes;
5, oven dry
Base line after the above-mentioned dehydration is sent into K031 type hot air type reeled yarn drying machine, and bake out temperature is 88 ℃, and drying time 40 minutes obtains knitting wool.
Embodiment 5
1, base line
With 70 kilograms of milk fibres, 40 kilograms of silks, 24 kilograms of sky silks, 66 kilograms of wools mix, and make bar on spinning equipment, it are sent into spinning machine again and make the base line;
2, wash line
Above-mentioned base line is sent into GM372 molded lines belt four groove tape machines to be washed;
3, dyeing
The above-mentioned base line of having washed is sent into dye vat for 100 kilograms, add 3500 kg of water; The dyeing machine running, add acetic acid, making the dye liquor pH value is 5.2, turns round to add 4 kilograms of glauber salt, 0.6 kilogram of dispersant and 1.5 kilograms of levelling agents after 5 minutes, rerun adding 0.02 kilogram of weak acid blue 7BF, 0.28 kilogram of pake purpke FBL of faintly acid after 5 minutes, rerunned 30 minutes; Temperature raise 1 ℃ in per 3 minutes in the dye vat then, rose to 60 ℃; Add the grand pake purpke 3BLH of 0.07 kilogram calorie magnetic, insulation running 10 minutes; Temperature raise 1 ℃ in per 4 minutes in the dye vat then, rose to 95 ℃, insulation running 30 minutes; Spilling water is cooled to 35 ℃, adds 2 kilograms of acetic acid and 5 kilograms of softener mixed liquors, and the insulation running is 20 minutes again, goes out cylinder;
4, dehydration
The above-mentioned base line that dyed look is sent into Z751-1200 type centrifugal type Water Extraction Machinery, dewatered 10 minutes;
5, oven dry
Base line after the above-mentioned dehydration is sent into K031 type hot air type reeled yarn drying machine, and bake out temperature is 90 ℃, and drying time 40 minutes obtains knitting wool.
Embodiment 6
1, base line
52 kilograms of milk fibres, 148 kilograms of wools are mixed, on spinning equipment, make bar, again it is sent into spinning machine and make the base line;
2, wash line
Above-mentioned base line is sent into GM372 molded lines belt four groove tape machines to be washed;
3, dyeing
The above-mentioned base line of having washed is sent into dye vat for 100 kilograms, add 3800 kg of water; The dyeing machine running adds acetic acid, and making the dye liquor pH value is 5.5, turns round to add 10 kilograms of glauber salt, 1.5 kilograms of dispersants and 3 kilograms of levelling agents after 5 minutes, reruns 0.5 kilogram of acid light yellow of adding after 5 minutes, reruns 30 minutes; Temperature raise 1 ℃ in per 4 minutes in the dye vat then, rose to 75 ℃; Add 0.1 kilogram of cationic yellow 8GL, insulation running 20 minutes; Temperature raise 1 ℃ in per 6 minutes in the dye vat then, rose to 100 ℃, insulation running 50 minutes; Spilling water is cooled to 40 ℃, adds 3 kilograms of acetic acid and 8 kilograms of softener mixed liquors, and the insulation running is 30 minutes again, goes out cylinder;
4, dehydration
The above-mentioned base line that dyed look is sent into Z751-1200 type centrifugal type Water Extraction Machinery, dewatered 10 minutes;
5, oven dry
Base line after the above-mentioned dehydration is sent into K031 type hot air type reeled yarn drying machine, and bake out temperature is 95 ℃, and drying time 40 minutes obtains knitting wool.
Embodiment 7
1, base line
40 kilograms of milk fibres, 60 kilograms of sky silks, 60 kilograms of wools, 40 kilograms of cottons are mixed, on spinning equipment, make bar, again it is sent into spinning machine and make the base line;
2, wash line
Above-mentioned base line is sent into GM372 molded lines belt four groove tape machines to be washed;
3, dyeing
The above-mentioned base line of having washed is sent into dye vat for 100 kilograms, put into 3000 kg of water; The dyeing machine running, add 6 kilograms and prevent being stained with agent, turn round and add 1 kilogram of levelling agent after 5 minutes, rerunned 5 minutes, and added 0.25 kilogram of ten thousand moral reactive golden yellow 4RFN, 0.25 kilogram of ten thousand moral reactive red 2BF, rerun 15 kilograms of glauber salt of adding after 10 minutes, after rerunning 10 minutes, add 15 kilograms of glauber salt again, rerun 7.5 kilograms of soda ash of adding in 10 minutes, rerunned 10 minutes; Temperature raise 1 ℃ in per 1 minute in the dye vat then, rose to 50 ℃, and insulation running 5 minutes adds 7.5 kilograms of soda ash, and the insulation running is 20 minutes again; Spilling water is cooled to 20 ℃, emptying then; In the dye vat of above-mentioned emptying, put into 3000 kg of water; The dyeing machine running adds 1 kilogram of acetic acid, and every running added 0.5 kilogram of dispersant, 0.5 kilogram of levelling agent, 0.45 kilogram of this golden yellow RL of pleasure, 0.05 kilogram of this dark red BR of pleasure in 5 minutes successively, rerunned 30 minutes; Raise 1 ℃ in per 2 minutes in the dye vat then, rise to 50 ℃, adds 0.01 kilogram of cationic yellow 8GL, 0.008 kilogram of cationic red GRL, 0.002 kilogram of Cationic Pure Blue GB, insulation was turned round 5 minutes; Temperature in the dye vat raise 1 ℃ in per again 2 minutes, rose to 90 ℃, insulation running 20 minutes; Spilling water is cooled to 30 ℃, adds 1 kilogram of acetic acid and 3 kilograms of softener mixed liquors, and insulation running 30 minutes goes out cylinder;
4, dehydration
The above-mentioned base line that dyed look is sent into Z751-1200 type centrifugal type Water Extraction Machinery, dewatered 10 minutes;
5, oven dry
Base line after the above-mentioned dehydration is sent into K031 type hot air type reeled yarn drying machine, and bake out temperature is 86 ℃, and drying time 40 minutes obtains knitting wool.
Embodiment 8
1, base line
48 kilograms of milk fibres, 40 kilograms of cottons, 112 kilograms of wools are mixed, on spinning equipment, make bar, again it is sent into spinning machine and make the base line;
2, wash line
Above-mentioned base line is sent into GM372 molded lines belt four groove tape machines to be washed;
3, dyeing
The above-mentioned base line of having washed is sent into dye vat for 100 kilograms, put into 3000 kg of water; The dyeing machine running, add 12 kilograms and prevent being stained with agent, turn round and add 2 kilograms of levelling agents after 5 minutes, rerunned 5 minutes, and added 0.8 kilogram of ten thousand moral reactive turquoise blue BGFN, rerun 24 kilograms of glauber salt of adding after 10 minutes, after rerunning 10 minutes, add 24 kilograms of glauber salt again, rerun 15 kilograms of soda ash of adding in 10 minutes, rerunned 10 minutes; Temperature raise 1 ℃ in per 31 minutes in the dye vat then, rose to 60 ℃, and insulation running 8 minutes adds 15 kilograms of soda ash, and the insulation running is 25 minutes again; Spilling water is cooled to 30 ℃, emptying then; 3600 kg of water in the dye vat of above-mentioned emptying adds; The dyeing machine running adds 2 kilograms of acetic acid, and every running added 4 kilograms of glauber salt, 1 kilogram of dispersant, 1 kilogram of levelling agent, 0.21 kilogram of this emerald green blue 5GMA of pleasure, 0.49 kilogram of this blue 2RLA of pleasure in 5 minutes successively, rerunned 30 minutes; Raise 1 ℃ in per 3 minutes in the dye vat then, rise to 60 ℃, adds 0.03 kilogram of Cationic Pure Blue GB, insulation was turned round 13 minutes; Temperature in the dye vat raise 1 ℃ in per again 3 minutes, rose to 96 ℃, insulation running 40 minutes; Spilling water is cooled to 36 ℃, adds 2 kilograms of acetic acid and 5 kilograms of softener mixed liquors, and insulation running 30 minutes goes out cylinder;
4, dehydration
The above-mentioned base line that dyed look is sent into Z751-1200 type centrifugal type Water Extraction Machinery, dewatered 10 minutes;
5, oven dry
Base line after the above-mentioned dehydration is sent into K031 type hot air type reeled yarn drying machine, and bake out temperature is 91 ℃, and drying time 40 minutes obtains knitting wool.
Embodiment 9
1, base line
56 kilograms of milk fibres, 144 kilograms of cottons are mixed, on spinning equipment, make bar, again it is sent into spinning machine and make the base line;
2, wash line
Above-mentioned base line is sent into GM372 molded lines belt four groove tape machines to be washed;
3, dyeing
The above-mentioned base line of having washed is sent into dye vat for 100 kilograms, put into 3000 kg of water; The dyeing machine running, add 18 kilograms and prevent being stained with agent, turn round and add 3 kilograms of levelling agents after 5 minutes, rerunned 5 minutes, and added 2 kilogram of ten thousand moral reactive brilliant yellow 4GLN, 1 kilogram of ten thousand moral reactive dark blue 2GLN, rerun 45 kilograms of glauber salt of adding after 10 minutes, after rerunning 10 minutes, add 45 kilograms of glauber salt again, rerun 22.5 kilograms of soda ash of adding in 10 minutes, rerunned 10 minutes; Temperature raise 1 ℃ in per 4 minutes in the dye vat then, rose to 70 ℃, and insulation running 10 minutes adds 22.5 kilograms of soda ash, and the insulation running is 30 minutes again; Spilling water is cooled to 40 ℃, emptying then; 4000 kg of water in the dye vat of above-mentioned emptying adds; The dyeing machine running adds 4 kilograms of acetic acid, and every running added 10 kilograms of glauber salt, 2 kilograms of dispersants, 2 kilograms of levelling agents, 0.17 kilogram of this golden yellow RL of pleasure in 5 minutes successively, and 0.83 kilogram of this dark red BR of pleasure rerunned 30 minutes; Raise 1 ℃ in per 4 minutes in the dye vat then, rise to 70 ℃, adds 0.007 kilogram of cationic yellow 8GL, 0.042 cationic red GRL, 0.001 kilogram of grand pake purpke 3BLH of long magnetic, insulation was turned round 20 minutes; Temperature in the dye vat raise 1 ℃ in per again 4 minutes, rose to 100 ℃, insulation running 60 minutes; Spilling water is cooled to 40 ℃, adds 3 kilograms of acetic acid and 8 kilograms of softener mixed liquors, and insulation running 30 minutes goes out cylinder;
4, dehydration
The above-mentioned base line that dyed look is sent into Z751-1200 type centrifugal type Water Extraction Machinery, dewatered 10 minutes;
5, oven dry
Base line after the above-mentioned dehydration is sent into K031 type hot air type reeled yarn drying machine, and bake out temperature is 94 ℃, and drying time 40 minutes obtains knitting wool.

Claims (7)

1, a kind of preparation method who contains the knitting wool of milk fibre is characterized in that, preparation method's step is:
A. base line
Base line raw material components and percentage by weight consist of:
Milk fibre 20-35%,
One of it silk, wool, silk, cotton, cashmere or be combined as 65-80% arbitrarily,
Base line needed raw material is carried out stripping on spinning equipment, again it is sent into spinning machine and make the base line;
B. wash line
Above-mentioned base line is sent into tape machine to be washed;
C. dyeing
The dyeing of base line after the above-mentioned washing can be adopted one of one-bath dyeing, one-bath two-step process dyeing or two one-bath two-step process dyeings; Its bath raio is 1: 30-40;
(1) use one-bath dyeing, the component of dyestuff and be to the percentage by weight of base line:
1) weak acid dye 0.01-0.1%,
2) the acetic acid pH value of transferring dye liquor to 4-6,
3) levelling agent 0.8-2%,
4) glauber salt 0-10%,
5) mixed liquor of acetic acid 1-3% and softener 2-8%,
One-bath dyeing step: the required above-mentioned base line of having washed is sent into dye vat, add required water by bath raio; Dyeing machine running adds required acetic acid, and every then running adds required levelling agent and glauber salt, weak acid dye successively after 5 minutes, rerunned 30 minutes; Raise 1 ℃ in the every 1-4 of temperature minute in the dye vat then, rise to 85 ℃, raise 1 ℃ in every again 1-3 minute, be raised to 90-100 ℃, insulation running 20-40 minute; Spilling water is cooled to 30-40 ℃, adds the mixed liquor of required acetic acid and softener, and the insulation running is 10-30 minute again, goes out cylinder;
(2) with one-bath two-step process dyeing, the component of dyestuff and be to the percentage by weight of base line:
1) 0.1-0.5% of weak acid dye,
2) 0.05-0.1% of cation dyes,
3) the acetic acid pH value of transferring dye liquor to 5-5.5,
4) glauber salt 0-10%,
5) dispersant 0.3-1.5%,
6) levelling agent 1-3%,
7) mixed liquor of acetic acid 1-3% and softener 3-8%,
One-bath two-step process staining procedure: the required above-mentioned base line of having washed is sent into dye vat, add required water by bath raio; The dyeing machine running adds required acetic acid, turns round to add required glauber salt, dispersant and levelling agent after 5 minutes, reruns 5 minutes, adds weak acid dye, reruns 30 minutes; In the dye vat the every 2-4 of temperature minute then, raise 1 ℃, rise to 50-75 ℃; Add cation dyes, insulation running 5-20 minute; Temperature raise 1 ℃ in every again 2-6 minute in the dye vat then, rose to 90-100 ℃, was incubated 20-50 minute; Spilling water is reduced to 30-40 ℃, adds the mixed liquor of required acetic acid and softener, and the insulation running is 10-30 minute again, goes out cylinder;
(3) use two one-bath two-step process dyeings, first bath when dyeing dye component and be to the percentage by weight of base line or the weight that adds by every premium on currency in the dye vat:
1) cotton reactive dye 0.5-3%,
2) glauber salt 10-30g/L,
3) soda ash 5-15g/L,
4) anti-be stained with agent 2-6g/L,
5) levelling agent 1-3%,
The first bath staining procedure is sent the required above-mentioned base line of having washed into dye vat, adds required water by bath raio; The dyeing machine running, add the required anti-agent of being stained with, turn round and add required levelling agent after 5 minutes, rerunned 5 minutes, and added required cotton reactive dye, rerun after 10 minutes and to add 1/2 of required glauber salt weight, rerun 1/2 other glauber salt of adding after 10 minutes, rerunned 10 minutes, and added 1/2 of required soda ash weight, rerunned 10 minutes; Raise 1 ℃ in the every 1-4 of temperature minute in the dye vat then, rise to 50-70 ℃, insulation running 5-10 minute adds other 1/2 soda ash, and the insulation running is 20-30 minute again; Spilling water is cooled to 20-40 ℃, emptying then;
The component of second dyestuff when bathing two steps dyeing and be to the percentage by weight of base line:
1) weak acid dye 0.5-1%,
2) cation dyes 0.02-0.05%,
3) acetic acid 1-4%,
4) glauber salt 0-10%,
5) dispersant 0.5-2%,
6) levelling agent 0.5-2%,
7) mixed liquor of acetic acid 1-3% and softener 3-8%,
Second bathes the step of two steps dyeing: add entry again by bath raio in the dye vat of above-mentioned emptying; The dyeing machine running adds required acetic acid, and every running adds required glauber salt, dispersant, levelling agent, weak acid dye successively after 5 minutes, rerunned 30 minutes; Raise 1 ℃ in the every 2-4 of temperature minute in the dye vat then, rise to 50-70 ℃, adds required cation dyes, insulation was turned round 5-20 minute; Temperature raise 1 ℃ in every again 2-4 minute in the dye vat, rose to 90-100 ℃, insulation running 20-60 minute; Spilling water is cooled to 30-40 ℃, adds the mixed liquor of required acetic acid and softener, and insulation running 30 minutes goes out cylinder;
D. dehydration
The above-mentioned base line that dyed look is sent into Water Extraction Machinery, dewatered 10 minutes;
The e oven dry
Base line after the above-mentioned dehydration is sent into dryer, and bake out temperature is 85-95 ℃, dries and obtains knitting wool after 40 minutes.
2, the preparation method who contains the knitting wool of milk fibre as claimed in claim 1 is characterized in that, bath raio is 1: 37-40.
3, the preparation method who contains the knitting wool of milk fibre as claimed in claim 2 is characterized in that, wherein uses one-bath dyeing, the component of dyestuff and be to the percentage by weight of base line:
1) weak acid dye 0.06-0.1%,
2) the acetic acid pH value that transfers to dye liquor to 5.3-6,
3) levelling agent 1.1-2%,
4) glauber salt 5-10%,
5) acetic acid 1-2% (O, W, f) and the mixed liquor of softener 4-8%.
4, the preparation method who contains the knitting wool of milk fibre as claimed in claim 1 is characterized in that, wherein with one-bath two-step process dyeing, and the component of dyestuff and be to the percentage by weight of base line:
1) weak acid dye 0.3-0.5%,
2) cation dyes 0.07-0.1%,
3) the acetic acid pH value of transferring dye liquor to 5.2-5.5,
4) glauber salt 4-10%,
5) dispersant 0.6-1.5%,
6) levelling agent 1-1.5%,
7) acetic acid 1-2% (O, W, f) and the mixed liquor of softener 5-8%.
5, the preparation method of the knitting wool of milk fibre as claimed in claim 1 is characterized in that, wherein uses two one-bath two-step process dyeings, first bath when dyeing dye component and be to the percentage by weight of base line or the weight that adds by every premium on currency in the dye vat:
1) cotton reactive dye 0.8-3%,
2) glauber salt 16-30g/L,
3) soda ash 10-15g/L,
4) anti-be stained with agent 4-6g/L,
5) levelling agent 2-3%.
6, the preparation method who contains the knitting wool of milk fibre as claimed in claim 1 is characterized in that, wherein bathes the dyeing of two steps with two, the component of second dyestuff when bathing two steps dyeing and be to the percentage by weight of base line:
1) weak acid dye 0.7-1%,
2) cation dyes 0.03-0.05%,
3) acetic acid 2-4%,
4) glauber salt 4-10%,
5) dispersant 1.1-2%,
6) levelling agent 1-2%,
7) mixed liquor of acetic acid 1-2% and softener 5-8%.
7, as the knitting wool of one of the preparation method of the described knitting wool that contains milk fibre of claim 1-6 preparation.
CN200510011736A 2005-05-18 2005-05-18 Method for preparing wool comprising milk protein fiber and wool thereby Expired - Fee Related CN100580164C (en)