WO1997014750A1 - Method for producing water-dispersible resin, and aqueous coating composition containing it - Google Patents

Method for producing water-dispersible resin, and aqueous coating composition containing it Download PDF

Info

Publication number
WO1997014750A1
WO1997014750A1 PCT/JP1996/002987 JP9602987W WO9714750A1 WO 1997014750 A1 WO1997014750 A1 WO 1997014750A1 JP 9602987 W JP9602987 W JP 9602987W WO 9714750 A1 WO9714750 A1 WO 9714750A1
Authority
WO
WIPO (PCT)
Prior art keywords
water
molecule
epoxy resin
resin
quaternary ammonium
Prior art date
Application number
PCT/JP1996/002987
Other languages
French (fr)
Inventor
Katsue Nishikawa
Youshichi Hagiwara
Original Assignee
W.R. Grace & Co. - Conn.
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by W.R. Grace & Co. - Conn. filed Critical W.R. Grace & Co. - Conn.
Priority to AU73324/96A priority Critical patent/AU7332496A/en
Publication of WO1997014750A1 publication Critical patent/WO1997014750A1/en

Abstract

The object of the present invention is to provide a stable water-dispersible resin, using a reduced amount of an organic solvent or not using any organic solvent, and to provide an aqueous coating composition comprising the water-dispersible resin and capable of forming on metallic substrates a protective film having excellent characteristics. The invention provides a method for preparing a water-dispersing resin comprising: (1) preparing an aqueous dispersion of a modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule, from an epoxy resin having a least two 1,2-epoxy groups in one molecule and having an epoxy equivalent of from 100 to 5,000, (2) polymerizing, in the aqueous dispersion, at least one unsaturated monomer component that indispensably comprises an unsaturated compound having at least one unsaturated group and at least one carboxyl group in one molecule, and (3) adding to the resulting polymer from 0.2 to 3.0 moles, per carboxyl equivalent of the polymer, of ammonia, a primary amine, a secondary amine, a tertiary amine or an inorganic alkaline substance to thereby neutralize the carboxyl groups of the polymer.

Description

DESCRIPTION METHOD FOR PRODUCING WATER-DISPERSIBLE RESIN, AND AQUEOUS COATING COMPOSITION CONTAINING IT
TFΓHNTΓ&T, FT T.ΓI
The present invention relates to a coating composition for metallic substrates. More precisely, it relates to an aqueous coating composition which is useful as a coating composition for forming a protective film on the inside and outside of metallic cans, or as a coating composition for precoated metal sheets that are generally referred to as precoat metals. R&ΓIΓΓ;T?OTTNΓJ APT * Various coating compositions are applied to the inside and the outside of metallic cans for canned (or tinned) goods and also to metallic substrates themselves to be formed into metallic cans, in order to prevent the metals from being corroded by the contents, to prevent the metals from dissolving into the contents and to prevent the outside prints from being damaged. In addition, various coating compositions are also used for repairing the damaged coats as formed during the production of coated cans. For these purposes, heretofore, coating compositions comprising epoxy resins and curing agents for the resins and vinyl-type coating compositions have been popularly used, as having excellent adhesion to metallic substrates, excellent corrosion resistance and excellent flavor characteristics. These epoxy-type coating compositions and vinyl-type coating compositions are prepared by dissolving the constitutive components in organic solvents.
In producing coated metallic cases, precoated metal sheets may be worked in order to obviate the need for coating the shaped cases later. Precoated metal sheets to be used for this purpose are referred to as precoat metals.
Recently, in view of environmental problems, pollution caused by the vaporization of organic solvents and about the health and safety of workers, the conversion of various organic solvent-type coating compositions into aqueous coating compositions has been promoted. This applies also to coating compositions for metals. For example, there have heretofore been developed compositions to be prepared by grafting an epoxy resin with an acrylic polymer having carboxyl groups, then neutralizing the carboxyl groups in the resin with an alkali, and dispersing the resin in water, such as those disclosed in Japanese Patent Laid-Open No. 63-178691 and Japanese Patent Publication No. 59- 37287; coating compositions to be prepared by neutralizing a reaction product of an epoxy resin and a polymer having carboxyl groups with an alkali, followed by dispersing it in water, such as those disclosed in Japanese Patent Publication Nos. 63-41934 and 59-37026; and compositions to be prepared by dispersing an epoxy resin and a curing agent for the resin in water along with an emulsifier of an acrylic polymer having carboxyl groups, such as those disclosed in Japanese Patent Application Laid-Open No. 63-275675.
However, the aqueous coating compositions as obtained according to the methods mentioned above are problematic in that they are poorly stable and that the production of these requires high temperatures, long-time reaction steps and hardly- controllable reaction conditions. In addition, after the preparation of the compositions, the organic solvent existing therein is removed in order to reduce the organic solvent content of the compositions. This results in still other problems in that the production costs increase and that the organic solvent vaporizes during the process of removing it. nτsrτ.osτmκ OF TM F.NTTnrj The present invention has been made in order to solve the above-mentioned problems, and its object is to provide a water- dispersible resin which can be produced with a significantly reduced amount of an organic solvent and from which, even when formulated into a coating composition, the removal of the organic solvent is unnecessary, and also to provide an aqueous coating composition comprising the resin, which has good storage stability and exhibits good flavor characteristics, adhesiveness, boiling water resistance and workability when used as a coating composition for metals. Specifically, the present invention relates to a method for preparing a water-dispersible resin, which comprises (1) preparing an aqueous dispersion of a modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule, from an epoxy resin having at least two 1,2-epoxy groups in one molecule and having an epoxy equivalent of from 100 to 5,000, (2) polymerizing, in the aqueous dispersion, at least one unsaturated monomer component that indispensably comprises an unsaturated compound having at least one unsaturated group and at least one carboxyl group in one molecule, and (3) adding to the resulting polymer from 0.2 to 3.0 moles, per carboxyl equivalent of the polymer, of ammonia, a primary amine, a secondary amine, a tertiary amine or an inorganic alkaline substance to thereby neutralize the carboxyl groups of the polymer. The invention also relates to an aqueous coating composition comprising the water-dispersible resin.
In the method of the present invention, any and every known epoxy resin having at least two 1,2-epoxy groups in one molecule and having an epoxy equivalent of from 100 to 5,000 can be employed. Examples of the epoxy resin include glycidyl ether- type epoxy resins such as typically bisphenol A-type epoxy resins, and glycidyl polycarboxylates, glycidylamine-type epoxy resins, linear aliphatic epoxy resins, alicyclic epoxy resins, and novolak-type epoxy resins. These epoxy resins can be used singly or as mixtures of two or more.
In the method of the present invention, commercially- available epoxy resins such as those mentioned above can be directly used, but can also be used after having been modified under heat with epoxy resin modifiers. One example of the modification is to modify an epoxy resin having two terminal 1,2- epoxy groups in one molecule to thereby increase its molecular weight to that of a higher polymer. As examples of epoxy resin modifiers to be used for this purpose of increasing the molecular weight of an epoxy resin into a higher polymer, mentioned are bisphenols such as bisphenol A, bisphenol F; vegetable oil fatty acids such as soybean oil fatty acids, dehydrated castor oil, tall oil fatty acids; dimer acids; and mixtures of these. If desired, aromatic carboxylic acids, such as benzoic acid and p- tert-benzoic acid, can also be used together with the modifiers. In addition, a part of the epoxy groups in the epoxy resin having at least two 1,2-epoxy groups in one molecule and having an epoxy equivalent of from 100 to 5,000 can be reacted with a higher fatty acid, such as stearic acid, palmitic acid or stearic acid, to thereby improve the flexibility of the resin.
In the first step of the method of the present invention that is to prepare an aqueous dispersion of a modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule, from an epoxy resin having at least two 1,2- epoxy groups in one molecule and having an epoxy equivalent of from 100 to 5,000, for example, the epoxy resin is first reacted with a tertiary amine to thereby convert the epoxy groups into quaternary ammonium hydroxide groups, and then reacted with an organic acid to thereby convert the quaternary ammonium hydroxide groups into quaternary ammonium carboxylate groups, and the resulting modified epoxy resin is dispersed in water.
Accordingly, the first aspect of the present invention is a method for preparing a water-dispersible resin comprising the steps of:
(a) reacting an epoxy resin having at least two 1,2-epoxy groups in one molecule and having an epoxy equivalent of from 100 to 5,000 with from 1 to 1.5 equivalents, per equivalent of the epoxy resin, of a tertiary amine, in the presence of water in a solvent, to prepare a modified epoxy resin having at least two quaternary ammonium hydroxide groups in one molecule;
(b) reacting the modified epoxy resin having at least two quaternary ammonium hydroxide groups in one molecule as obtained in the previous step (a) with an organic acid having at least one carboxyl group in one molecule to prepare a modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule;
(c) dispersing in water the modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule as obtained in the previous (b) ;
(d) polymerizing, in the aqueous dispersion of the modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule as obtained in the previous step (c), at least one unsaturated monomer component that indispensably comprises an unsaturated compound having at least one unsaturated group and at least one carboxyl group in one molecule; and - (e) adding to the resulting polymer from 0.2 to 3.0 moles, per carboxyl equivalent of the polymer, of ammonia, a primary amine, a secondary amine, a tertiary amine or an inorganic alkaline compound, to thereby neutralize the carboxyl groups in the polymer. In the method of the first aspect of the present invention mentioned above, an epoxy resin having at least two 1,2-epoxy groups in one molecule is first reacted with a tertiary amine in the presence of water in a solvent, thereby converting the terminal epoxy groups of the epoxy resin into quaternary ammonium hydroxide groups, to prepare a modified epoxy resin having at least two quaternary ammonium hydroxide groups in one molecule, in the step (a). This reaction can be represented by the following chemical reaction formula: -CH-CH9 +
Y 2 NR1R2R3
Figure imgf000009_0001
Examples of the tertiary amine that shall be used for this purpose include trimethylamine, triethylamine, dimethylethanol- amine, methyldiethanolamine, ethylmethylethanolamine, dimethyl- ethylamine, dimethylpropylamine, dimethyl-3-hydroxy-1-propyl- amine, dimethylbenzylamine; and mixtures of these amines. The reactional ratio between the tertiary amine and the 1,2-epoxy groups in the epoxy resin is desirably such that the ratio of epoxy grou /tertiary amine is from 1.0/1.0 to 1.0/1.5. If the amount of the tertiary amine is not more than this range, the tertiary amine will act as the polymerization catalyst to cause the polymerization of the epoxy groups, thereby often gelling the reaction product during the reaction. If, however, it is over the range, the excess amount of the amine remains in the product and neutralizes the carboxyl group-containing polymer that shall be added later to the reaction system, whereby the reaction of converting the quaternary ammonium hydroxide groups into quaternary ammonium carboxylate groups will be retarded or the product will have an offensive amine-like odor.
The reaction of the epoxy resin with the tertiary amine to produce quaternary ammonium hydroxide groups is conducted generally at a temperature falling between 5β C and 100"C, after the epoxy resin has been dissolved in a suitable solvent. If the temperature is lower than 5βC, the reaction could not be promoted and will take much time. If it is higher than 100βC, some undesirable side reactions will occur and the reaction product may gel.
Any and every known organic solvent capable of dissolving epoxy resins can be used for the reaction of the epoxy resin with the tertiary amine. Desirably, however, used are alcoholic solvents capable of dissolving both the starting epoxy resin and the quaternary ammonium hydroxide produced. Such alcoholic solvents include, for example, cellosolve solvents such as methyl cellosolve, ethyl cellosolve, and butyl cellosolve; diethylene glycol solvents such as carbitol, and butyl carbitol; and monoesters of propylene glycol. The unsaturated monomer component that shall be used as the reactant in the following step of the method of the present invention can also be used as the reaction solvent for the reaction of the epoxy resin with the tertiary amine.
The reaction time necessary for the formation of the quaternary ammonium hydroxide varies, depending on the epoxy resin used, the tertiary amine used, the organic solvent used, the concentration of the reactants in the organic solvent, and the reaction temperature. In general, however, it may be from 5 minutes to 12 hours.
In the method of the present invention, the organic solvent is required only in the step (a) of reacting the epoxy resin with the tertiary amine or in another step of reacting the epoxy resin with the tertiary amine and an organic acid that shall be mentioned hereinunder. Accordingly, by minimizing the amount of the organic solvent to be used in this stage, the organic solvent content of the final product can be reduced. A suitable amount of the organic solvent to be used varies, depending on the molecular weight of the epoxy resin used, but may well be such that the solvent can completely dissolve the epoxy resin to give an epoxy resin solution capable of being stirred and reacted at predetermined reaction temperatures. The amount of the solvent may be generally such that the epoxy resin solution can have a resin concentration of from 60 to 90 % by weight. The reaction for converting the terminal epoxy groups of the epoxy resin into quaternary ammonium hydroxide groups is promoted more rapidly, if the reactant concentration is higher or, that is, the concentration of the epoxy resin solution is higher. From this viewpoint, it is desirable to reduce the amount of the organic solvent to be used. As has been mentioned hereinabove, the unsaturated monomer component that shall be used as a reactant in the following step of the method of the present invention can also be used as the solvent to dissolve the epoxy resin. If the monomer is used in this manner, no organic solvent is used in the method of the present invention. Thus, an absolute aqueous resin can be produced.
Water is indispensable in the step (a) of the method of the invention of forming the quaternary ammonium hydroxide groups. The amount of water necessary for the formation of the quaternary ammonium hydroxide groups in the invention may be satisfactorily brought by water in air that shall be taken into the reactor and thus into the reaction system during the reaction, or by water to be contained in the epoxy resin, the tertiary amine and the organic solvent to be used. In general, however, it is desirable to add water to the reaction system in an amount of 30 times by weight or less of the tertiary amine used in the reaction. Addition of too much water over this range to the reaction system is unfavorable, as it retards the reaction. In the next step (b), an organic acid having at least one carboxyl group in one molecule is added to the modified epoxy resin having at least two quaternary ammonium hydroxide groups in one molecule, thus obtained in the previous step (a), to thereby attain the ion exchange between the quaternary ammonium hydroxide group and the carboxyl group to give a different modified epoxy resin having quaternary ammonium carboxylate groups.
The ion exchange reaction between the quaternary ammonium hydroxide group and the carboxyl group can be represented by the following chemical reaction formula:
Figure imgf000012_0001
The organic acid having at least one carboxyl group in one molecule, which is used in the step (b) of the method of the present invention, includes, for example, aliphatic mono¬ carboxylic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, oleic acid, and lactic acid; aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, azelaic acid, and sebacic acid; aromatic carboxylic acids such as benzoic acid, toluic acid, and naphthoic acid; and mixtures of two or more of these. However, such are not limitative.
As examples of the organic acid having at least one carboxyl group in one molecule that are especially preferably used in the method of the present invention, mentioned are unsaturated carboxylic acids capable of being further polymerized after having acted on the quaternary ammonium hydroxide groups to convert them into the quaternary ammonium carboxylate groups. Such unsaturated carboxylic acids include, for example, acrylic acid, methacrylic acid, crotonic acid, isocrotonic acid, itaconic acid, fumaric acid, maleic acid, citraconic acid, and succinic acid.
The amount of the organic acid to be used shall be from 0.3 to 6.0 moles, per mole of the quaternary ammonium hydroxide groups as converted from the terminal hydroxyl groups of the epoxy resin. If the amount of the organic acid used is less than this range, it is difficult to disperse the quaternary ammonium carboxylates formed in water. If, however, it is over the range, the characteristics, especially the water-resistance of the film to be finally formed from the aqueous coating composition comprising the resin will be lowered.
In the method of the present invention, the reaction of the modified epoxy resin having quaternary ammonium hydroxide groups as derived from the epoxy resin with the organic acid having at least one carboxyl groups in one molecule to produce the different modified epoxy resin having quaternary ammonium carboxylate groups can be attained merely by mixing the two at room temperature. However, in order to further ensure the mixing and the reaction of the two, it is more desirable to heat and stir the reaction system at from room temperature to 100°C for from 5 minutes to 2 hours.
Apart from the above-mentioned process of the invention for converting the epoxy groups of the epoxy resin into the quaternary ammonium carboxylate groups via the quaternary ammonium hydroxide groups, it is also possible to employ a one- step process of reacting an epoxy resin having at least two 1,2- epoxy groups in one molecule and having an epoxy equivalent of from 100 to 5,000 with both a tertiary amine and an organic acid such as those mentioned hereinabove to produce the quaternary ammonium carboxylate groups.
Accordingly, the second aspect of the present invention is a method for producing a water-dispersible resin comprising the steps of:
(i) reacting an epoxy resin having at least two 1,2-epoxy groups in one molecule and having an epoxy equivalent of from 100 to 5,000 with from 1 to 1.5 equivalents, per equivalent of the epoxy resin, of a tertiary amine and an organic acid, in the presence of water in a solvent, to prepare a modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule;
(ii) dispersing in water the modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule as obtained in the previous step (i);
(iii) polymerizing, in the aqueous dispersion of the modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule as obtained in the previous step (ii), at least one unsaturated monomer component that indispensably comprises an unsaturated compound having at least one unsaturated group and at least one carboxyl group in one molecule; and (iv) adding to the resulting polymer from 0.2 to 3.0 moles, per carboxyl equivalent of the polymer, of ammonia, a primary amine, a secondary amine, a tertiary amine or an inorganic alkaline compound, to thereby neutralize the carboxyl groups in the polymer. The process of this second embodiment requires reaction conditions that are different from those for the reaction of forming the quaternary ammonium hydroxide in the process of the first aspect of the invention mentioned above. Specifically, in the above-mentioned step (i) of the process of the second aspect of the invention, it is necessary to add both a tertiary amine and an organic acid to the epoxy resin as dissolved in a suitable organic solvent and to heat and stir them at a temperature falling between 60"C and 120βC for from 30 minutes to 12 hours. This reaction can be represented by the following chemical reaction formula: CH-CH2 + NRjR^ + RCOOH
Figure imgf000015_0001
Regarding the type and the amount of the solvent to be used in this reaction, referred to are those mentioned hereinabove. In the method of the present invention, the solution of the quaternary ammonium carboxylate thus formed in the manner as mentioned above is thereafter dispersed in water, to which is added an unsaturated monomer component. In this process, the unsaturated monomer component to be subjected to polymerization in the next step may be added to the solution of the quaternary ammonium carboxylate prior to dispersing the carboxylate solution in water, or, alternatively, the solution of the quaternary ammonium carboxylate is first dispersed in water and thereafter the monomer component may be added to and dispersed in the aqueous dispersion of the quaternary ammonium carboxylate.
The amount of water to be used for the aqueous dispersion shall be determined, depending on the use and the object of the aqueous coating composition to be finally obtained herein and on the coating system to be applied to the composition. In general, however, the amount of water in question may well be such that the solid content of the coating composition can be from 10 to 80 % by weight.
The unsaturated monomer component to be added to the system of the present invention shall comprise an unsaturated compound having at least one unsaturated group in one molecule. The unsaturated compound includes, for example, acrylates and methacrylates such as methyl acrylate, methyl methacrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, n-hexyl methacrylate, and lauryl methacrylate; unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, isocrotonic acid, itaconic acid, fumaric acid, maleic acid, citraconic acid, and cinnamic acid; and vinyl monomers such as acrylamide, styrene, vinyl acetate, and acrylonitrile. In general, two or more of them are combined in consideration of the stability of the aqueous coating composition to be finally obtained herein and of the characteristics of the cured film to be formed from the composition. In the present invention, it is indispensable that at least one unsaturated monomer to be polymerized comprises an unsaturated carboxylic acid having at least one carboxyl group and at least one unsaturated group in one molecule. The amount to be used of the unsaturated carboxylic acid having at least one carboxyl group and at least one unsaturated group in one molecule has a great influence on the dispersibility in water of the resin to be obtained, and the rheology thereof. In the method of the present invention, the relationship between the amount to be used of the unsaturated carboxylic acid having at least one carboxyl group and at least one unsaturated group in one molecule and the dispersibility in water of the resin to be obtained depends on the molecular weight of the starting epoxy resin from which the modified epoxy resin having quaternary ammonium hydroxide groups is derived. However, in order to obtain a resin having good dispersibility in water, the amount of the unsaturated carboxylic acid to be used must be such that the carboxyl content of the acid is from 1.5 to 6.0 times by mole of the quaternary ammonium hydroxide content of the epoxy resin. If the amount is less than this range, it is difficult to obtain a resin with good dispersibility in water and to obtain an aqueous coating composition with good storage stability. If, on the other hand, the amount is over the range, the characteristics, especially the water-resistance of the cured film to be formed from the coating composition are poor.
Next, a radical polymerization initiator is added to the thus-obtained aqueous dispersion comprising the modified epoxy resin having quaternary ammonium carboxylate groups and the unsaturated monomer component comprising indispensably an unsaturated compound having at least one carboxyl group and at least one unsaturated group in one molecule, and then heated, whereby the unsaturated compound in the aqueous dispersion is polymerized. The polymerization is effected generally at a temperature falling between 50*C and 100"C for from 15 minutes to 3 hours. In order to efficiently promote it, the polymerization is preferably effected in an inert gas stream, such as nitrogen or argon. The radical polymerization initiator to be employed herein includes, for example, peroxides such as benzoyl peroxide, and lauroyl peroxide, as well as azobisisobutyronitrile, 2,2'- azobis(2,4-dimethylvaleronitrile) , potassium persulfate, and ammonium persulfate, which, however, are not limitative. In addition, also employable are redox initiators, such as a combination of hydrogen peroxide and a ferrous salt, and a combination of a persulfate and acidic sodium sulfite.
In the method of the present invention, the unsaturated compound having at least one carboxyl group and at least one unsaturated group in one molecule is neutralized at the carboxyl group in the molecule, with ammonia, a primary amine, a secondary amine, a tertiary amine or an inorganic alkaline substance, during or after the polymerization. We, the present inventors have found that, when a radical polymerization initiator is added to the aqueous dispersion of the quaternary ammonium carboxylate and the unsaturated compound having at least one unsaturated group in one molecule, and heated to polymerize the unsaturated compound in the dispersion, then an epoxy resin grafted with a carboxyl-containing acrylic polymer via a quaternary ammonium group, such as that shown in the following formula, is formed, the resin thus formed is essentially insoluble in water and therefore coagulates during the polymerization, and the resulting coagulate changes to a water-dispersible resin if neutralized with an amine or an alkali. As a result of these findings, we have completed the present invention. Specifically, after having found that, if an alkali is added to the polymerization system, after the formation of the coagulate, to thereby re-disperse the coagulate, or if an alkali is added thereto at the initial stage of the formation of the coagulate or, that is, in the course of the polymerization, it is possible to obtain a stable, water- dispersible resin, we have completed the present invention.
epoxy resin-CH-CH9 —N+
OH RlR?R3 COOH COOH
The alkaline substance to be employed herein for this purpose includes, for example, ammonia; primary amines such as monomethylamine, monoethylamine, n-butylamine, sec-butylamine, and n-amylamine; secondary amines such as dimethylamine, diethyl¬ amine, di-n-butylamine, dioctylamine, and diethylenetriamine; tertiary amines such as trimethylamine, triethylamine, tri- isopropanolamine, ethyldiethanolamine, dimethylethanolamine, and triethanolamine; aniline, morpholine, toluidine, and pyridine; and also inorganic alkalis such as sodium hydroxide, potassium hydroxide, lithium hydroxide, and sodium carbonate. However, these are not limitative. The amount of the alkaline substance to be added is from 0.2 to 3.0 moles per mole of the carboxyl group in the polymer to be obtained through the above-mentioned polymerization. If the amount is less than this range, it is impossible to obtain a stable water-dispersible resin. If, however, it is over the range, the excess alkaline substance will cause the storage stability of the aqueous coating composition comprising the resin to deteriorate or will have a negative influence on the characteristics of the film to be finally obtained from the composition. - The water-dispersible resin thus obtained in the manner as mentioned hereinabove can be used even singly as an aqueous coating material to exhibit sufficient coating characteristics. However, in order to obtain a tougher film using the resin, it is desirable to add to the resin a curing agent of a phenolic resin or an amino resin.
The amino resin capable of being added to the resin of the invention includes, for example, partially butylated or methylated melamine, hexamethoxymethylmelamine, hexaethoxymethyl- melamine, benzoguanamine, butylated benzoguanamine, aceto- guanamine, partially or wholly butylated urea, triazine derivatives, and mixtures of these. The phenolic resin capable of being used as the curing agent in the present invention includes, for example, phenol-formaldehyde resins, resol-type phenolic resins, novolak-type phenolic resins, bisphenol A-type resol resins, and partially butyl-etherified phenolic resins. Also employable as the curing agent is a reaction product of phenol or cresol with formaldehyde. If the curing agent is used, its amount to be added is preferably from 3 to 50 % by weight relative to the solid content of the aqueous coating composition comprising the water- dispersible resin. If the amount is less than this range, the characteristics, especially the hot water-resistance of the coating film to be obtained will be often poor. If, on the other hand, it is over the range, it is difficult to obtain a stable, aqueous coating composition comprising the water-dispersible resin.
The aqueous coating composition comprising the water- dispersible resin of the present invention can be applied to metallic substrates either directly or, if desired, after having formed an undercoat on the substrates, or after having shaped the substrates, according to any known coating method of, for example, roll coating, spray coating, dip coating, or brush coating. The thickness of the coating film to be formed from the composition is not specifically defined, provided that the metallic substrates are uniformly coated with the composition. The preferred thickness of the coating film may be generally from 1 to 50 μm, though it varies depending on the use and the object of the metallic substrates coated.
After having been applied to metallic substrates, the aqueous coating composition of the present invention is thermally cured at a temperature falling between 80"C and 240" C for from 1 to 30 minutes. If the curing temperature is lower than this range, the film cannot be completely cured so that it cannot attain the object of protecting the metallic substrates. If, on the other hand, it is over the range, the properties of the film to be finally obtained are worsened and the metallic substrates are deteriorated. TNΓ>TTSTPTAT. APPT.TΓARTT.TTV
As has been described hereinabove, it is possible, according to the present invention, to prepare a stable water-dispersible resin while using a reduced amount of an organic solvent or not using any organic solvent, and also to provide an aqueous coating composition comprising the water-dispersible resin, which can form on metallic substrates a protective film having excellent characteristics. - The present invention is described in more detail hereinunder with reference to the following examples, which, however, are not intended to restrict the scope of the present invention.
FYAMPT.FS (Example 1) Production of Water-Dispersible Resin
200 g (0.1 equivalents) of a bisphenol A-type epoxy resin, YD-017 (epoxy equivalent=1927, produced by Toto Chemicals Co.) was dissolved in 86 g of n-butoxyethanol. Next, 9.3 g (0.1 moles) of dimethylethanolamine and 10 g of water were added thereto and reacted for 3 hours at 60" C, thereby converting the epoxy groups in the epoxy resin into quaternary ammonium hydroxide groups. 30 g (0.42 moles) of acrylic acid was added to the solution of the quaternary ammonium hydroxide-containing modified epoxy resin, and stirred for 30 minutes at 80" C thereby converting the jjuaternary ammonium hydroxide groups into quaternary ammonium carboxylate groups. Next, 38 g of methyl methacrylate and 20 g of ethyl acrylate were added thereto, and stirred, and then 586 g of water was added thereto. Thus was obtained a semi-transparent, aqueous dispersion of quaternary ammonium carboxylate-containing modified epoxy resin/acrylic monomer. As a polymerization initiator, 1 g of 2,2' -azobis(2,4- dimethylvaleronitrile) was added to the resulting aqueous dispersion, which was then subjected to polymerization at 80"C in a nitrogen stream. 40 minutes after the addition of the polymerization initiator, 30 ml of aqueous 28 % ammonia was added to this, with which the carboxyl groups therein were neutralized. After polymerization for 1 hour at 80"C, obtained was a stable water-dispersible resin. Even after having been stored at room temperature for 1 month or longer, the water-dispersible resin thus obtained gave neither precipitate nor coagulate of the resin component. (Example 2) Production of Water-Dispersible Resin 100 g (0.05 equivalents) of a bisphenol A-type epoxy resin, YD-017 (epoxy equivalent=1927, produced by Toto Chemicals Co.) was dissolved in 60 g of n-butoxyethanol. Next, 5.0 g (0.056 moles) of dimethylethanolamine and 10 g of water were added thereto, stirred at room temperature, and then left static at room temperature for 10 hours. Thus was obtained a solution of a quaternary ammonium hydroxide-containing modified epoxy resin. 5.1 g (0.056 moles) of lactic acid was added to the solution, and stirred for 30 minutes at 70"C, thereby converting the quaternary ammonium hydroxide groups in the modified resin into quaternary ammonium carboxylate groups. Next, 270 g of water was added to this, which gave an almost transparent dispersion. 20 g of methyl methacrylate, 10 g of ethyl acrylate and 12 g of acrylic acid were added to this dispersion, and 1.3 g of a polymerization initiator, 2,2'-azobis(2,4-dimethylvaleronitrile) was added thereto and subjected to polymerization at 80"C in a nitrogen stream. After one hour, a coagulate was formed in the system. 12 g of dimethylethanolamine was added thereto, by which the coagulant was wholly re-dispersed to give a creamy, water- dispersible resin having low viscosity. As in Example 1, the resin dispersion obtained herein was stable. (Example 3) Production of Water-Dispersible Resin
100 g (0.056 equivalents) of a bisphenol a-type epoxy resin, Epicoat 1007 (epoxy equivalent=1789, produced by Yuka Shell Co.) was dissolved in 67 g of carbitol, and 5 g (0.056 moles) of dimethylethanolamine and 10 g of water were added thereto, and stirred for 3 hours at 50"C to obtain a solution of a quaternary ammonium hydroxide-containing modified epoxy resin. To this solution was added 15.8 g (0.18 moles) of methacrylic acid and stirred for 1 hour at 60"C, whereby the quaternary ammonium hydroxide groups in the modified resin were converted into quaternary ammonium carboxylate group. Next, 180 g of water was added thereto, and 0.5 g of a polymerization initiator, 2,2'- azobis(2,4-dimethylvaleronitrile) was added thereto, and subjected to polymerization at 80" C in a nitrogen stream. 30 minutes after the start of the polymerization, 8 g of aqueous 28 % ammonia was added to the reaction system, and the polymerization was continued further. After one hour, obtained was a white aqueous dispersion of a water-dispersible resin. (Example 4) Production of Water-Dispersible Resin
200 g (0.08 equivalents) of a bisphenol A-type epoxy resin, YD-019 (epoxy equivalent=2467, produced by Toto Chemicals Co.) was dissolved in 120 g of n-butoxyethanol. Next, 7.1 g (0.08 moles) of dimethylethanolamine and 15 g of water were added thereto, and reacted for 3 hours at 60"C to obtain a solution of a quaternary ammonium hydroxide-containing modified epoxy resin. 5.0 g of acetic acid was added to this solution, and stirred for 30 minutes at 80" C to thereby convert the quaternary ammonium hydroxide groups in the modified resin into quaternary ammonium carboxylate groups. Next, 433 g of water was added thereto, and an almost transparent dispersion was obtained. 38 g of methyl methacrylate, 20 g of ethyl acrylate and 22 g of acrylic acid were added to this dispersion, and 1.3 g of a polymerization initiator, 2,2'-azobis(2,4-dimethylvaleronitrile) was added thereto and subjected to polymerization at 80" C in a nitrogen stream. After one hour, a coagulate was formed in the system. 15 g of aqueous 28 % ammonia was added thereto, by which the coagulant was wholly re-dispersed to give a creamy, water- dispersible resin having low viscosity. As in Example 1, the resin dispersion obtained herein was stable. (Example 5) Production of Water-Dispersible Resin 200 g (0.1 equivalents) of a bisphenol A-type epoxy resin, YD-017 (epoxy equivalent=1927, produced by Toto Chemicals Co.) was dissolved in 134 g of n-butoxyethanol. Next, 9.7 g (0.11 moles) of dimethylethanolamine and 10 g of water were added thereto and reacted for 3 hours at 60" C, thereby converting the epoxy groups in the epoxy resin into quaternary ammonium hydroxide groups. 30 g (0.42 moles) of acrylic acid was added to the solution of the quaternary ammonium hydroxide-containing modified epoxy resin, and stirred for 30 minutes at 80" C thereby converting the quaternary ammonium hydroxide groups into quaternary ammonium carboxylate groups. Next, 58 g of methyl methacrylate was added thereto, and stirred, and then 484 g of water was added thereto. Thus was obtained a semi-transparent, aqueous dispersion of quaternary ammonium carboxylate group- containing modified epoxy resin/acrylic monomer. As a polymerization initiator, 1 g of 2,2' -azobis(2,4-dimethylvalero- nitrile) was added to the resulting aqueous dispersion, which was then subjected to polymerization at 80" C in a nitrogen stream. 20- minutes after the addition of the polymerization initiator, a solution as prepared by dissolving 20 ml of aqueous 28 % ammonia in 40 ml of water was added to this, with which the carboxyl groups therein were neutralized. After polymerization for 1 hour at 80"C, obtained was a stable water-dispersible resin. Even after having been stored at room temperature for 1 month or longer, the aqueous dispersion of the resin thus obtained gave neither any precipitate nor any coagulate. (Example 6) Production of Water-Dispersible Resin
80 g (0.032 equivalents) of a bisphenol A-type epoxy resin, YD-019 (epoxy equivalent=2477, produced by Toto Chemicals Co.) was dissolved in 57 g of n-butoxyethanol. To this were added 2.3 g of acrylic acid, 2.9 g of dimethylethanolamine, 0.6 g of water, and 0.002 g of p-methoxyhydroquinone, and reacted for 2 hours at 90" C. Next, 292 g of water was added thereto to obtain a semi¬ transparent dispersion. 16 g of methyl methacrylate and 8.5 g of methacrylic acid were added to this dispersion, and 1 g of a polymerizationinitiator,2,2'-azobis(2,4-dimethylvaleronitrile) was added thereto, and subjected to polymerization at 80" C in a nitrogen stream.
After one hour, the reaction product coagulated. When 8.0 g of dimethylethanolamine was added thereto, the coagulate was wholly re-dispersed to give a stable water-dispersible resin. (Comparative Example 1)
200 g (0.1 equivalents) of a bisphenol A-type epoxy resin, YD-017 (epoxy equivalent=1927, produced by Toto Chemicals Co.) was dissolved in 86 g of n-butoxyethanol. Next, 9.3 g (0.1 moles) of dimethylethanolamine and 10 g of water were added thereto, and reacted for 3 hours at 60"C, thereby converting the epoxy groups in the resin into quaternary ammonium hydroxide groups. 38 g of methyl methacrylate and 20 g of ethyl acrylate were added to the solution of the quaternary ammonium hydroxide- containing modified epoxy resin thus obtained, and stirred, and then 586 g of water was added thereto. However, the quaternary ammonium hydroxide-containing modified epoxy resin was not dispersed in water. From this, it is understood that the conversion of the quaternary ammonium hydroxide groups in the resin into quaternary ammonium carboxylate groups with an acid is indispensable in order to obtain a resin with good dispersibility in water. (Comparative Example 2) Production of Water-Dispersible Resin 200 g (0.1 equivalents) of a bisphenol A-type epoxy resin. YD-017 (epoxy equivalent=1927, produced by Toto Chemicals Co.) was dissolved in 134 g of n-butoxyethanol. Next, 9.7 g (0.11 moles) of dimethylethanolamine and 10 g of water were added thereto, and reacted for 3 hours at 60" C, thereby converting the epoxy groups in the resin into quaternary ammonium hydroxide groups. 30 g (0.42 moles) of acrylic acid was added to the solution of the quaternary ammonium hydroxide-containing modified epoxy resin thus obtained, and stirred for 30 minutes at 80" C, thereby converting the quaternary ammonium hydroxide groups in the modified resin into quaternary ammonium carboxylate groups. Next, 58 g of methyl methacrylate was added thereto, and stirred, and then 484 g of water was added thereto to obtain a semi¬ transparent aqueous dispersion of quaternary ammonium carboxylate group-containing modified epoxy resin/acrylic monomer. A solution as prepared by dissolving 20 ml of aqueous 28 % ammonia in 40 ml of water was added to the resulting aqueous dispersion to thereby neutralize the carboxyl groups therein, whereupon the dispersion immediately coagulated just after the addition of the aqueous ammonia thereto and the reaction could not be continued further more.
(Comparative Example 3)
200 g (0.1 equivalents) of a bisphenol A-type epoxy resin, YD-017 (epoxy equivalent=1927, produced by Toto Chemicals Co.) was dissolved in 86 g of n-butoxyethanol. Next, 9.3 g (0.1 moles) of dimethylethanolamine and 10 g of water were added thereto, and reacted for 3 hours at 60° C, thereby converting the epoxy groups in the resin into quaternary ammonium hydroxide groups. 30 g of acrylic acid was added to the solution of the quaternary ammonium hydroxide-containing modified epoxy resin thus obtained, and stirred for 30 minutes at 80"C, thereby converting the quaternary ammonium hydroxide groups in the modified resin into quaternary ammonium carboxylate groups. Next, 38 g of methyl methacrylate and 20 g of ethyl acrylate were added thereto, and stirred, and then 1 g of a polymerization initiator, 2,2' -azobis(2,4-dimethylvaleronitrile) was added to this, which was thus subjected to polymerization at 80"C in a nitrogen stream. Ten minutes after the start of the polymerization, the reaction product gelled. (Comparative Example 4)
80 g (0.03 equivalents) of a bisphenol A-type epoxy resin, YD-019 (epoxy equivalent=2497, produced by Toto Chemicals Co.) was dissolved in 53 g of n-butoxyethanol. Next, 2.8 g (0.031 moles) of dimethylethanolamine and 0.6 g of water were added thereto, and reacted for 1 hour at 80" C to obtain a solution of a quaternary ammonium hydroxide-containing modified epoxy resin. To this solution was added 2.0 g (0.033 moles) of acetic acid, and stirred for 30 minutes at 80" C thereby converting the quaternary ammonium hydroxide groups in the modified resin into quaternary ammonium carboxylate groups. Next, 374 g of water was added thereto to obtain a semi-transparent dispersion. To this were added 10.2 g of methyl methacrylate and 6.8 g of n-butyl acrylate, and 1 g of a polymerization initiator, 2,2' -azobis(2,4- dimethylvaleronitrile) was added to this, which was thus subjected to polymerization at 80"C in a nitrogen stream. After having been reacted for 30 minutes at 80"C, this gave a semi- transparent dispersion. Since the viscosity of the dispersion thus obtained was too low, it was difficult to use it as a coating material.
(Example 7) Preparation of Aqueous Coating Compositions and Evaluation of Their Properties
The water-dispersible resins as obtained in Examples 1 and 5 were directly used as coating materials, or each were combined with the curing agent as shown in Table 1 and formulated into aqueous coating compositions. The amount of the curing agent added was 10 % by weight relative to the solid resin content of each water-dispersible resin. In addition, the water-dispersible resin as obtained in Comparative Example 4 was directly used as a coating material, or was formulated into an aqueous coating composition in the same manner as above. These resin compositions each were applied onto a tin plate, using a wire bar, at a dry film thickness of 10 μm, and then cured at 200"C for 12 minutes.
To determine the degree of curing thereof, each sample was subjected to a rubbing test up to 100 cycles, in which the sample was rubbed two times with a cotton soaked with methyl ethyl ketone (MEK) in one cycle. The number of cycles after which the film was damaged was counted. To determine the adhesiveness of each film to the plate, each sample was subjected to a so-called cross-cut tape-peeling test, in which cross-cuts of 1 mm were formed on the film with a cutter knife, and an adhesive cellophane tape was attached thereto and then peeled off. The adhesiveness was evaluated according to 6-rank evaluation, in which "0" indicates that the film was not peeled along with the adhesive tape, and "5" indicates that the film was completely peeled. In addition, each coated sample was subjected to a boiling test, in which it was left in an autoclave at 131"C for 30 minutes whereupon the condition of the outward appearance of the coating film was observed. The test results are shown in Table 1.
Table 1
Water- MEK Cross-Cut Boiling
Dispersible Curing Agent Resistance Tape-Peeling Resistance
Resin Test
Example 1 No >100 0 No Change
Example 1 SFC 099 >100 0 No Change
Example 1 Cymel 303 >100 0 No Change
Example 5 No >100 0 No Change
Example 5 PR-217 >100 0 No Change
Comparative No 1 - - Example 4
Comparative Cymel 303 2 - - Example 4
SFC 099: Phenolic Resin, produced by Schenectady Co. Cymel 303: Hexamethoxymethylolmelamine, produced by Mitsui Cyanamid Co. PR-217: Phenolic Resin, produced by Hoechst AG.

Claims

CLAIMS 1. A metho for preparing a water-dispersible resin comprising the steps of:
(a) reacting an epoxy resin having at least two 1,2-epoxy groups in one molecule and having an epoxy equivalent of from
100 to 5,000 with from 1 to 1.5 equivalents, per equivalent of the epoxy resin, of a tertiary amine, in the presence of water in a solvent, to prepare a modified epoxy resin having at least two quaternary ammonium hydroxide groups in one molecule;
(b) reacting the modified epoxy resin having at least two quaternary ammonium hydroxide groups in one molecule as obtained in the previous step (a) with an organic acid having at least one carboxyl group in one molecule to prepare a modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule;
(c) dispersing in water the modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule as obtained in the previous (b); (d) polymerizing, in the aqueous dispersion of the modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule as obtained in the previous step (c), at least one unsaturated monomer component that indispensably comprises an unsaturated compound having at least one unsaturated group and at least one carboxyl group in one molecule; and
(e) adding to the resulting polymer from 0.2 to 3.0 moles, per carboxyl equivalent of the polymer, of ammonia, a primary amine, a secondary amine, a tertiary amine or an inorganic alkaline compound, to thereby neutralize the carboxyl groups in the polymer.
2. A method for preparing a water-dispersible resin comprising the steps of:
(i) reacting an epoxy resin having at least two 1,2-epoxy groups in one molecule and having an epoxy equivalent of from 100 to 5,000 with from 1 to 1.5 equivalents, per equivalent of the epoxy resin, of a tertiary amine and an organic acid, in the presence of water in a solvent, to prepare a modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule;
(ii) dispersing in water the modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule as obtained in the previous step (i);
(iii) polymerizing, in the aqueous dispersion of the modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule as obtained in the previous step (ii), at least one unsaturated monomer component that indispensably comprises an unsaturated compound having at least one unsaturated group and at least one carboxyl group in one molecule; and
(iv) adding to the resulting polymer from 0.2 to 3.0 moles, per carboxyl equivalent of the polymer, of ammonia, a primary amine, a secondary amine, a tertiary amine or an inorganic alkaline compound, to thereby neutralize the carboxyl groups in the polymer.
3. The method for preparing a water-dispersible resin as claimed in claim 1, wherein the organic acid to be used in the step (b) is an unsaturated carboxylic acid having both at least one unsaturated group and at least one carboxyl group in one molecule.
4. The method for preparing a water-dispersible resin as claimed in claim 2, wherein the organic acid to be used in the step (i) is an unsaturated carboxylic acid having both at least one unsaturated group and at least one carboxyl group in one molecule.
5. The method for preparing a water-dispersible resin as claimed in claim 1 or 2, wherein at least one unsaturated monomer component that indispensably comprises an unsaturated compound having at least one unsaturated group and at least one carboxyl group in one molecule is added to the modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule, then water is added to the resulting mixture to prepare an aqueous dispersion of the mixture, and the aqueous dispersion is subjected to polymerization.
6. The method for preparing a water-dispersible resin as claimed in claim 1 or 2, wherein the modified epoxy resin having at least two quaternary ammonium carboxylate groups in one molecule is dispersed in water, then at least one unsaturated monomer component that indispensably comprises an unsaturated compound having at least one unsaturated group and at least one carboxyl group in one molecule is added to the resulting dispersion, and the dispersion thus obtained is subjected to polymerization.
7. The method for preparing a water-dispersible resin as claimed in claim 1 or 2, wherein from 0.2 to 3.0 moles, per carboxyl equivalent of the polymer, of ammonia, a primary amine, a secondary amine, a tertiary amine or an inorganic alkaline compound is added to the reaction system in the course of polymerization, to thereby neutralize the carboxyl groups of the polymer.
8. The method for preparing a water-dispersible resin as claimed in claim 1 or 2, wherein from 0.2 to 3.0 moles, per carboxyl equivalent of the polymer, of ammonia, a primary amine, a secondary amine, a tertiary amine or an inorganic alkaline compound is added to the reaction system after polymerization, to thereby neutralize the carboxyl groups of the polymer.
9. An aqueous coating composition comprising a water- dispersible resin as produced in the method of claim 1 or 2, along with a phenolic resin or an amino resin.
PCT/JP1996/002987 1995-10-16 1996-10-16 Method for producing water-dispersible resin, and aqueous coating composition containing it WO1997014750A1 (en)