USRE25451E - Prevention of development of color by - Google Patents

Prevention of development of color by Download PDF

Info

Publication number
USRE25451E
USRE25451E US25451DE USRE25451E US RE25451 E USRE25451 E US RE25451E US 25451D E US25451D E US 25451DE US RE25451 E USRE25451 E US RE25451E
Authority
US
United States
Prior art keywords
color
polyvinyl chloride
asbestos
iron
composition
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired
Application number
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Publication date
Application granted granted Critical
Publication of USRE25451E publication Critical patent/USRE25451E/en
Expired legal-status Critical Current

Description

United States Patent 1 25,451 PREVENTION OF DEVELOPMENT OF COLOR BY lRON COMPOUNDS IN PLASTICS Arthur C. Hacker, Bronx, and Mark W. Pollock, Forest Hills, N.Y., assignors to Argus Chemical Corporation, a corporation of New York No Drawing. Original No. 2,943,070, dated June 28, N60, Ser. No. 689,503, Oct. 11, 1957. Application for reissue July 30, 1962, Ser. No. 214,177 Claims. (Cl. 26023) Matter enclosed in heavy brackets appears in the original patent but forms no part of this reissue specification; matter printed in italics indicates the additions made by reissue.
This invention relates to bleaching colored iron compounds in plastics and, in another embodiment, to preventing development of the color of such compounds initially. The invention is particularly applicable in the manufacture of pigmented fioor tile containing thermoplastic material and will be first illustrated by description in connection with such use.
It is customary in making the floor tile to use polyvinyl plastic with a fibrous reinforcing agent and a large proportion of pigment of which calcium carbonate in finely divided form is representative. When the reinforcing agent is a material such as a purified asbestos, the resulting floor tile retains its original established color, which is White to gray when the pigment is calcium carbonate, without substantial discoloration during hot compounding or a couple of hours or more of subsequent heat testing at 300 F. When, however, there is incorporated an iron compound or when the asbestos is used in the unpurified state containing a normal content of iron compounds, then there is developed, during heating as at 300 F, a purple to bluish gray color that is very pronounced even after 15 minutes heating.
We have now discovered that, when the composition including the iron containing asbestos is compounded in usual manner as by rolling at a stock temperature of about 275 F. for minutes and the purple to bluish gray discoloration is so developed, introducing our special protecting agent, here actually a bleaching agent, and then subjecting the recompounded material to the heating test at 300 F. for 2 hours causes bleaching of the original purple. The bleaching is pronounced in 5 minutes and the color becomes lighter as the heating continues. This is in contrast to the increase in color ordinarily obtained with various plastic compositions, subject to heat discoloration, as the period of heating is lengthened.
Likewise we have found that incorporation of our protective agent at the beginning of the compounding or milling operation prevents the development of the discoloration referred to, without the need of any additional heating period to bleach the color that would otherwise have appeared.
Briefly stated, our invention comprises lloor tile or like article including a plastic, a source of hydrogen halide, an iron compound, and an agent protecting the iron from development of color on heating in contact with the other components of the composition.
The invention comprises also the use of the protecting agent as a color discharging material for lightening the color of a plastic composition of kind described that may have been discolored at an elevated temperature.
The plastic used is one containing a polyvinyl chloride, the term polyvinyl chloride being used herein to include resins consisting essentially of polyvinyl chloride (PVC) or copolymers thereof with vinyl acetate, vinylidene chlo ride and the like, the proportion of the PVC in the copolymers being -98 parts for 100 total weight of the copolymer and ordinarily about -95 parts. An example of such copolymer that we use is the commercial VYHH, a copolymer of 87 parts of vinyl chloride and 13 of vinyl acetate.
Iron-containing asbestos is the source of the iron compound, the asbestos used being any iron-containing variety although we actually use chrysotile asbestos. This asbestos contains both ferrous and ferric compounds, as for instance, about 0.1-5 parts of each calculated as ferrous oxide and ferric oxide, respectively, for of the asbestos and generally total iron calculated as ferric oxide within the range 2-8 parts.
The protecting agent used for its effect on color of the composition is one that is compatible with the selected plastic material at compounding temperatures and in the proportion used is substantially non-separating therefrom in eitlcr the hot condition of compounding or on cooling to atmospheric temperature. The agent is heat stable, that is not heat decomposable to a large extent, at the temperature of compounding. For permanent effect, it should have substantially no or only a low vapor pressure and, therefore, a slow rate of volatility at ordinary temperatures. Examples of materials that meet these requirements and that may be used are the organic polyols, poly as applied to the hydroxyl content meaning two or more alcoholic OH groups. Examples are the aliphatic polyhydroxy compounds such as trimethylolethane, pentaerythritol, sorbitol, mannitol, methyl glucoside, sucrose, hydroxy propylsuerose (hyprose) and their partial esters with any carboxylic acid, and polyhydroxy substituted acids such as gluconic, arabonic, and glucoheptoic acids and their lactones, salts, and esters, examples being (l -C alkyl esters and the sodium, potassium, and ammonium salts. Also we may use cyclo-aliphatic polyhydroxy compounds, examples of which are hydrogenated bisphenol A and base catalyzed condensation products of acetone or cyclohexanone with formaldehyde.
For improved maintenance of the physical properties of the composition we may and suitably do introduce also an epoxy compound such as epoxidized fatty glycetides, as for instance epoxidized soybean oil and other epoxidized higher fatty acid esters including the butyl, hexyl, octyl and glycol esters of oleic, linoleic, and like unsaturated acids; glycidyl ethers of phenols such as phenol itself, resorcinol and bisphenol A; and glycidyl ethers of the alcohols of which examples are the C -C monohydric alcohols such as lauryl, cyclohexyl and octadecyl and the polyhydric alcohols such as the C -C alkene diols, particularly ethylene, propylene, and butylene glycols, and glycerine.
The introduction of white pigments into the plastic, as in a pigmented vinyl resin floor tile, makes the effect of the protective agent more conspicuous than otherwise is the case. The pigment that We ordinarily use in the floor tile is finely divided calcium carbonate (Atomite). Other pigments that may be used are titanium dioxide, silica, and others that are conventional for this purpose and are selected to provide the color desired.
The applicants protecting agent is still required when the pigment used is one that is an antacid and would be expected, therefore, to neutralize any hydrogen chloride developed in the plastic composition during the compounding at elevated temperatures. Thus the protective agent is necessary when the plastic composition used is one containing, as the resin, polyethylene with a small proportion of ammonium chloride distributed therethroughout or when the resin selected is polyvinyl chloride, even though the pigment used may be a large proportion of the finely divided calcium carbonate.
The usual plasticizers are introduced, dioctyl phthalate or any of the epoxy compounds referred to above being ones commonly used. Additional plasticizers that may be used are dibutyl or dioctyl sebacate and tricresyl phosphate. The plasticizer must be a liquid compatible with the resin at compounding temperatures and non-separating therefrom in objectionable proportion at low winter temperatures. Also the plasticizer should be non-volatile or volatilizable only at a very slow rate at ordinary temperaturcs.
As to proportions, these, for the conventional materials, are those that are usual in products of the class to be made. Thus a commercial floor tile may contain the several components in about the proportions shown, satisfactory ranges of proportions being given in the parentheses: vinyl resin 100 parts, plasticizer 20 (15-60), asbestos 100 (25-200), calcium carbonate or other pigment 160 (10-200), protective agent 3 (l-lO), and epoxy compound 2 (-10). The proportions within these ranges will vary somewhat with the activity of the several components per unit or weight. The pigment, for example, will be low in proportion when it is one of exceptional hiding power. In the case of titanium dioxide, for instance, a suitable proportion is 12 parts for 100 of the resin. With the calcium carbonate pigment on the other hand, the proportion may be as high as 200 parts. Likewise the proportion of plasticizer is lower within the range stated when the plasticizer is one that is an active solvent for the vinyl resin and higher within the said range when it is a less elfective solvent for the vinyl resin.
As to conditions of manufacture, the protective agent may be used in one of two manners.
When used to discharge a color previously developed by action of the iron with a component of the hot compounded plastic composition, the protective agent is introduced near the end of the compounding operation. The compounding at the elevated temperatures such as 250- 300 F. is then continued until the purple or blue color originally developed has been bleached to about the white, gray, or other original color. When the protective agent is intended to avoid development of color initially, the agent is introduced into the composition before or at about the beginning of the compounding operation, that is, before there is any substantial period of hot-rolling or other mixing at the elevated temperature of compounding.
Ordinarily we effect the compounding of the polyethylene or PVC plastic with the asbestos, protective agent, and other components on the usual type of rubber mixing rolls, the temperature used being sulficient to cause compatibility of the various organic materials and sufficient flowability on the hot rolls to give uniform mixing.
The mixing by rolling or otherwise is continued until the composition becomes practically uniform, that is, the fibers of asbestos and the other components are mixed sufliciently uniformly to meet commercial standards. This requires ordinarily about to 30 minutes.
The invention will be further illustrated by detailed description in connection with the following specific examples of the practice of it. In these examples and elsewhere herein proportions are expressed as parts by weight.
4 EXAMPLE 1 In this example, the protective agent is pentaerythritol. Its effect was tested first on a polyvinyl chloride floor tile composition with white pigment, no iron being present in the asbestos or in other component of the composition. The etfect of the agent on discoloration, in compounding and in 2 hours subsequent heating of the shceted stock at 300 F., was completely negative.
When, how-ever, the commercial grade of asbestos containing iron was incorporated, in place of the purified, iron-free absestos, the effect of the pentaerythritol was exceedingly great. The specimens of the product retained practically the original color during all of the 2 hours heating, whereas specimens without the pentaerythritol turned to a purple after a 15-minute heating at 300 F. and to an intense blue-gray or blue-purple color in 30 minutes.
The more detailed information follows.
The basic plastic composition used for modification was of the following proportions:
Component Parts VYIIII (87% PVC-13% PVAc) DOI (dioctyl phthalatc plasticizcr) 18 Epoxidizcd soybean oil plasticizer 2. 5 TiO pigment 12 Color of Product Additive and Amount Product for 100 Parts VYIII-l 0n Conclusion After 2 hours Milling at 300 F.
A, Atomite (021003) 100 White White. B Pliwentaerthyritnbttdo Faint yellow. C Purified asbestos 100. Grayish white" Clrayish white. D C 4 .do Do. E Asbestos ((5% iron*)l0[) Light bluish Deep purple.
gray. F E+PE 4 Light gray.. Light gray. G C+Ferrous glucouato l. Grayish Wliito Bluish gray.
Total iron=2.7% ferrous and 3.3% ferric, both calculated as oxides.
The sample G shows the effect of iron added in form other than in the asbestos in also developing color in the 2-hour heating test.
Once the elfects described have been obtained, various theories may be advanced to explain the results. We consider that the withdrawal or otherwise prevention of iron from its usual reaction with other components of the plastic mixture, by the protective agent, is an important cause of the effects obtained. That the color developing reaction involves oxidation is indicated by the much more intense color developed on the faces of the samples E (Example 1), that were exposed to direct contact with air during the 2-hour heating, than on the back of the sample.
EXAMPLE 2 The basic stock in this example was a standard high pressure process polyethylene (DYNH) 100 parts, iron containing chrysotile asbestos (grade 7R) 50 parts, and titanium dioxide pigment 10. The stock after compounding alone was tested for 2 hours at 300 F. with observance of the color every 15 minutes. The basic stock was also modified during the compounding operation by the addition of other components as recorded in the table below and with the results shown.
(Dolor of Product Modifier and Product Amount for 100 Parts DYNH On Conclusion After 2 hours at of Milling 300 F.
H- None Grayish white Same.
Ammonion clilo- .(lo Faint Bluish cast.
ride 2. J Ammonium ehloclo Bluish east.
ride 10. K Ammonium ehlod Very faint yellow ride IO-l-PE 4. cost.
These results show the effect of 10% of ammonium chloride, a potential source of hydrogen chloride in causing the iron to be reactive in development of color, particularly in sample I. The effect of the small amount of protective agent, 4 parts of pentaerythritol, in preventing the development of purplish color is shown in sample K.
EXAMPLE 3 Col r of Sheeinrl Stock After 2 Hours at 3B0 F.
Polyol Used and Parts for 100 of the Rosin n-Butyl gluconato ti Hydroxy propylsucroso (L Hydrogenated Bisphenol A 12 Increased gray. Substantially uncharged. Increased gray.
The sucrose derivative used is Hyprose SP80.
EXAMPLE 4 The procedure of Example 3 was followed with additional polyols tested with the VYHH resin. It was found after 2 hours at 300 F. that methyl glucoside and sorbitol were more effective on an equal weight basis than pentaerythritol in protecting the iron compound from the undesired color development on heating in the VYHH at 300 F. for 2 hours.
EXAMPLE 5 The procedure of Example 1 with the composition of product E (asbestos containing iron) is followed with the substitution of the pentaerythritol separately and on an equal weight basis by each of the protective agents disclosed and not used in later examples and the substitution of the plasticizer separately by any other plasticizer dis closed lherein, also on an equal weight basis.
It is to be understood that it is intended to cover all changes and modifications of the examples of the invention herein chosen for the purpose of illustration which do not constitute departures from the spirit and scope of the invention.
The term consisting essentially of" as used in the claims renders the claims open only for the inclusion of unspecified ingredients which do not materially afiect the basic and novel characteristics of the composition, Ex parte Davis et al., 80 USPQ 448 at 450. The use of this term thereby excludes substances which materially change the fundamental inhibiting action of the organic polyhydroxy compound against discloration produced when polyvinyl chloride is heated in the presence of naturally occurring asbestos containing iron compounds. Substances which do not materially affect the inhibiting ootion of the polyhydroxy compound are not excluded from the claims and exemplary of nondeletcrious substances thus included are cpoxidized fatty glyceridcs.
This application is a continuation-in-part of Serial No. 403,072, new Patent No. 2,837,490.
We claim:
1. A polyvinyl chloride resin composition resistant when heated at elevated temperatures to the development of discoloration due to iron compounds present in asbestos as naturally-occurring, consisting essentially of a polyvinyl chloride resin, naturally-occurring asbestos containing iron compounds in an amount to discolor the polyvinyl chloride when heated, and an amount to iniibit such discoloration of a saturated organic polyhydroxy compound having at least two to about eight alcoholic hydroxyl groups for each two to about fifteen carbon atoms.
2. A polyvinyl chloride resin composition in accordance with claim 1 in which the polyhydroxy compound is a [polyhdric] polyhydric aliphatic alcohol.
3. A polyvinyl chloride resin composition in accordance with claim 2 in which the polyhydric alcohol is pentaerythritol.
4. A polyvinyl chloride resin composition in accordance with claim 2 in which the polyhydric alcohol is sorbitol.
5. A polyvinyl chloride resin composition in accordance with claim 1 [comprising] also containing an epoxidized fatty glyceride.
6. A polyvinyl chloride resin floor tile composition comprising a polyvinyl chloride resin composition in accordance with claim 1 and a pigment.
7. A polyvinyl chloride resin floor tile composition [comprising] consisting essentially of a polyvinyl chloride resin and, per parts of the polyvinyl chloride, from 10 to 200 parts of an inorganic pigment. from 25 to 20-0 parts of naturally-occurring asbestos containing iron compounds in an amount to discolor the polyvinyl chloride when heated and an amount to inhibit such discoloration of a saturated organic polyhydroxy compound having at least two to about eight alcoholic hydroxyl groups for each two to about fifteen carbon atoms.
8. A polyvinyl chloride resin fioor tile composition in accordance with claim 7 which in addition contains up to 10 parts of an epoxidized fatty glyceride.
9. A process of preparing an asbestos-containing polyvinyl chloride resin composition protected when heated against discoloration due to iron compounds present in the asbestos as naturally-occurring [which comprises] consisting essentially of including in the polyvinyl chloride resin composition an amount suflicicnt to inhibit such discoloration of a saturated organic polyhydroxy compound having at least two to about eight alcoholic hydroxyl groups for each two to about fifteen carbon atoms.
10. The process of bleaching a discolored polyvinyl chloride resin composition containing a colored compound formed by heating the composition at an elevated temperature in the presence of iron compounds contained in naturally-occurring asbestos, [which comprises] consisting essentially of incorporating in the discolored polyvinyl chloride resin composition a small amount of a saturated organic polyhydroxy compound having at least two to about eight alcoholic hydroxyl groups for each two to about fifteen carbon atoms and then heating at an elevated temperature until the color is lessened in intensity.
1]. A polyvinyl chloride resin composition in accordance with claim I also containing a glycidyl ether of a compound selected from the group consisting of phenols, monohydric alcohols having from six to eighteen carbon atoms, and dihydric alcohols having from two to eight carbon atoms.
12. A polyvinwl chloride resin composition in accordance with claim 5 in which the cpoxidizcd fatty glyccridc is cporirlizcd soy bean oil.
13. A polyvinyl chloride resin floor tile composition in accordance with claim 8 in which the epoxidized fatty glyceride is cpoxidized soy bean oil.
14. A process in accordance with claim 9 being further characterized by the inclusion in the polyvinyl chloride resin composition of an epoxidized fatty giyceride.
15. A process in accordance with claim 14 in which the epoxidizcd fatty giyccride is epoxidized soy bean oil.
References Cited in the file of this patent or the original patent UNITED STATES PATENTS 2,459,746 Radcliffe Jan. 18, 1949 8 Amberg Dec. 6, 1949 Lally et a1. Feb. 14, 1956 Hecker June 3, 1958 Elliott Nov. 18, 1958 Buckley et a1. Jan. 30, 1962 OTHER REFERENCES Shreve: Chemical Process Industries, 2nd edition, 0 pages 772-777, McGraw-Hill Book Co., 1956.
US25451D 1957-10-11 Prevention of development of color by Expired USRE25451E (en)