US20090285747A1 - Micro-domain graphitic materials and method for producing same - Google Patents

Micro-domain graphitic materials and method for producing same Download PDF

Info

Publication number
US20090285747A1
US20090285747A1 US12/266,577 US26657708A US2009285747A1 US 20090285747 A1 US20090285747 A1 US 20090285747A1 US 26657708 A US26657708 A US 26657708A US 2009285747 A1 US2009285747 A1 US 2009285747A1
Authority
US
United States
Prior art keywords
micro
graphitic
carbon
domain
reactor
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Abandoned
Application number
US12/266,577
Inventor
Steinar Lynum
Jan Hugdahl
Ketil Hox
Ragne Hildrum
Magne Nordvik
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
nTec AS
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Priority claimed from NO19971413A external-priority patent/NO313839B1/en
Application filed by Individual filed Critical Individual
Priority to US12/266,577 priority Critical patent/US20090285747A1/en
Publication of US20090285747A1 publication Critical patent/US20090285747A1/en
Assigned to AKER KVAERNER CARBON AS reassignment AKER KVAERNER CARBON AS ASSIGNMENT OF ASSIGNORS INTEREST (SEE DOCUMENT FOR DETAILS). Assignors: KVAERNER TECHNOLOGY & RESEARCH LTD
Assigned to AKER CARBON AS reassignment AKER CARBON AS CHANGE OF NAME (SEE DOCUMENT FOR DETAILS). Assignors: AKER KVAERNER CARBON AS
Assigned to N TEC AS reassignment N TEC AS ASSIGNMENT OF ASSIGNORS INTEREST (SEE DOCUMENT FOR DETAILS). Assignors: AKER CARBON AS
Abandoned legal-status Critical Current

Abstract

This invention relates to a method for producing micro-domain graphitic materials by use of a plasma process, and to novel micro-conical graphitic materials. By micro-domain graphitic material we mean fullerenes, carbon nanotubes, open conical carbon structures (also named micro-cones), preferably flat graphitic sheets, or a mixture of two or all of these. The novel carbon material is open carbon micro-cones with total disclination degrees of 60° and/or 120°, corresponding to cone angles of respectively 112.9° and/or 83.6°.

Description

  • This application is a continuation-in-part of prior application Ser. No. 09/400,530.
  • FIELD OF THE INVENTION
  • This invention relates to a method for producing micro-domain graphitic materials by use of a plasma process, and for producing novel micro-conical graphitic materials. By micro-domain graphitic materials we mean fullerenes, carbon nanotubes, open conical carbon structures (also named micro-cones), preferably flat graphitic sheets, or a mixture of two or all of these. The novel carbon material is open carbon micro-cones with total disclination degrees 60° and/or 120°, corresponding to cone angles of respectively 112.9° and/or 83.6°.
  • BACKGROUND OF THE INVENTION
  • There is currently an intense interest in novel carbon materials due to their unique and novel properties. For instance, the carbon materials may be useful to achieve high hydrogen energy storage, for use in purification processes as well as for different applications within the electrical/pharmaceutical sector. The properties are sensitive to the micro-structure of the carbon material, which can be varied by the degree of graphitisation and by introduction of rings other than hexagons in the network. Fullerenes are examples of novel graphitic structures where the introduction of a 12 pentagons in the hexagonal network results in closed shells (D. Huffman, Physics Today, p. 22, 1991). Carbon nanotubes are also an example of such possibilities (T. W. Ebbesen, Physics Today, p. 26, 1996). Open conical structures are yet another example of possible graphitic structures, but only three of five possible kinds have ever been synthesized (M. Ge and K. Sattler, Chemical Physics Letters, 220, P. 192, 1994; P. Li and K. Sattler, Mat. Res. Soc. Symp. Proc. 359, p. 87, 1995; R. Vincent, N. Burton, P. M. Lister and J. D. Wright, Inst. Phys, Conf. Ser. 138, p. 83, 1993).
  • Recent interest in fullerenes and nanotubes is amongst other connected to their use in the field of hydrogen storage. Hence, Fernando tubes a hydrogen storage of amazingly 75 wt % is reported (Hydrogen & Fuel Cell Letter, vol. 7/No. 2, February 1997) If this is the case, it will probably represent the break-through concerning a practical hydrogen storage system for use in the transportation sector. It is indicated that future fuel cell cars using this storage technology may achieve a range of about 8000 km.
  • In the case of fullerenes, more than 7 wt % of reversibly added hydrogen is achieved (R. M. Baum, Chem. Eng. News, 22, p. 8, 1993; Japanese Patent JP 27801 A2, Fullerene-based hydrogen storage media, 18th Aug. 1994; A. Hirsch, Chemistry of Fullerenes, Thieme Ferlag, Stuttgart, Ch. 5, p. 117, 1994). Fullerenes have also been used in a solid phase mixture with inter-metallic compounds or metals to achieve high contents of hydrogen, i.e. 24-26H atoms per fullerenes molecule (B. P. Tarasov, V. N. Fokin, A. P. Moravsky, Y. M. Shul'ga, V. A. Yartys, Journal of Alloys and Compounds 153-254, p. 25, 1997). Flat graphitic material formed of stacks of two-guy mention sheets has high surface area of for adsorption of guest elements and compounds. However, in such materials, the absorption process is limited by diffusion. The larger the graphitic domain, the slower the adsorption will be. Of potential interest would be highly graphitic eyes to materials where domains were small so that the guest material would readily reach all the graphitic micro domains by percolation through the bulk carbon material. The accessibility to the micro-domains could be further enhanced if some or all the domain is had been topple logical discrimination, preferably each domain having less or equal man 300 degrees disk letter nation to provide cavities, or micro-pores, for the flow of guest material.
  • A common problem with the present methods for synthesizing peas and graphitic materials is the little production yield. The fullerenes are most often synthesized by vapor rising graphite electrodes via carbon—are discharges in a reduced inner against atmosphere. There has been reported a conversion rate into fullerenes of 10-15%, corresponding to a generation rate of nearly 10 grams per hour (A. Hirsch, Chemistry of Fullerenes, Thieme Ferlag, Stuttgart, Ch. 5, p. 117, 1994).
  • The carbon-arc method is also the most frequently used method for production of carbon nanotubes. Nanotubes yields of about 60% of the core material have been obtained at optimal conditions (T. W. Ebbesen, Physics Today, p. 26, 1996). Still, the achieved yield is in gram quantities.
  • Small unspecified amount of open conical carbon and structures are obtained by resistively heating a carbon foil and further condensing the carbon vapor on a highly-oriented pyrolytic graphite surface (M. Ge and K. Sattler, Chemical Physics Letters, 220, P. 192, 1994; P. Li and K. Sattler, Mat. Res. Soc. Symp. Proc. 359, p. 87, 1995). The code angles produced by this method did was approximately 19° as well as 60° (P. Li and K. Sattler, Mat. Res. Soc. Symp. Proc. 359, p. 87, 1995). Resistive heating of a carbon rod, with further deposition on cooler surfaces was used to produce cones with apparent cone angles of approximately 39° (R. Vincent, N. Burton, P. M. Lister and J. D. Wright, Inst. Phys, Conf. Ser. 138, p. 83, 1993). It can be shown from a continuous sheet of graphite that only five types of cones can be assembled, where each domain is uniquely defined by its topological disclination TD given by the general formula:

  • TD=N×60 degrees, where N=0, 1, 2, 3, 4 or 5.
  • As used herein, the term “disclination” is defined as “a line defect arising from singularities in orientational order in a directional field”, which serves for further growth giving rotational symmetry. With respect to graphitic cones, these are created when a perfect graphitic plane with hexagons are interrupted by one or more pentagons. This results in a rotational fixture of the graphitic plane resulting in the start point of the cone, further symmetrical growth can follow from this. The disclination is defined to be the deviation angle from the hexagonal to a pentagon, that is 600 for 2 to 5 pentagons.
  • The structure of such graphitic domains can be grossly described as stacks of graphitic sheets with flat (N=0) or conical structures (N=1 to 5). Hence, two of these, holding cone angles of 83.6° and 112.9°, have not been reported so far.
  • SUMMARY OF THE INVENTION
  • An object of this invention is to provide a novel method for producing micro-domain graphitised materials. The method can give large yield rates, up to above 90%.
  • Another object of this invention is to provide a method that is suited for industrial scale production of micro-domain graphitised materials. Further, it is an object of this invention to provide a method that can produce a micro-domain graphitised materials which at least partly consists of a novel highly crystalline graphitic material composed of open conical carbon structures holding cone angles of 83.6° and 112.9°. This corresponds to N=1 and 2. The rest of the micro-conical graphitised materials are either fullerenes, carbon nanotubes, the other open carbon cones (N=3, 4, or 5), preferably flat graphitic sheets (N=0), or a mixture of two or more of these.
  • BRIEF DESCRIPTION OF THE DRAWINGS
  • FIG. 1 shows a schematic figure of the reactor and the surrounding equipment.
  • FIG. 2 shows a transmission electron microscope photograph of the samples revealing the various types of open micro-conical carbons of the invention.
  • FIG. 3 shows the projected angles for perfect graphitic cones, i.e. 19.2°, 38.9°, 60°, 83.6° and 112.9°, which represents total disclination of 300°, 240°, 180°, 120° and 60°, respectively. In addition a graphitic sheet, having a projected angle of 180° and a total disclination of 0°, is shown.
  • FIGS. 4A, 4B, 4C, 4D and 4E shows example of domains for each type of disclination 60°, 120°, 180°, 240° and 300°, respectively, present in the invention.
  • DETAILED DESCRIPTION OF THE EXEMPLARY EMBODIMENT
  • The invention is based upon decomposition of hydrocarbons into carbon and hydrogen in a plasma based process. The plasma are is formed in a plasma generator which consists of tubular electrodes, wherein the inner electrode is supplied with electrical direct voltage with one polarity and wherein the external electrode is connected to the opposite polarity from a power supply. The plasma generator is installed in connection with a decomposition reactor wherein the reactor is designed as a defined heat insulated chamber with an outlet for end products. The plasma gas is recycled from the process. Further description of the general process and the equipment is described in the applicant's Norwegian patent NO. 176522.
  • The structure of the resulting carbon material will depend on the following three process parameters: The hydrocarbon feed rate, the plasma gas enthalpy and the residence time. By varying these parameters the resulting carbon material will either be available as conventional carbon black, as micro-domain graphitic materials or a mixture of both. In this invention we will describe the process parameters for optimizing on micro-domain graphitic materials.
  • The hydrocarbons are introduced into a decomposition reactor and heated by a plasma gas in the vicinity of the plasma arc zone by use of a nozzle. The nozzle aligns the hydrocarbon spay in the axial direction of the reactor and is designed in such a way that coarse drops are formed. This is to prevail the hydrocarbon evaporation in such a way that the hydrocarbons start the cracking and polymerization process, which results in the formation of polycyclic aromatic hydrocarbons (PAHs). That is, the plasma gas enthalpy is controlled at such a level that the main fraction of the gaseous hydrocarbons does not reach the pyrolysis temperature at the specific speed rate and resistance time used. However, a small fraction of the gaseous hydrocarbons will inevitably reach the pyrolysis temperature and consequently react and convert to conventional carbon black.
  • The impurity fraction of carbon black would naturally be kept as low as possible, and is further, together with the wanted graphitic micro-domains, separated from the process gas containing the gaseous hydrocarbons (PAHs) by conventional filtering after exiting the reactor. A conventional filtering of a gas stream is assumed known to a skilled person and will not be further described here.
  • After the filtering of the process gas, the fraction of the process gas that contains the PAHs is reintroduced into the plasma torch once more as the plasma gas. When entering and going through the high energy intensive plasma arc zone of the plasma torch the second time, the gaseous PAHs will be fully converted to graphitic micro-domains. These micro-domains successively follow the heated plasma gas to the low temperature zone of the reactor and follow the process gas as explained above to the filter to be recovered as the product.
  • The reintroduction of the PAH-containing plasma gas can of course be performed by a recirculation loop (such as shown in FIG. 1) or by having two plasma reactors connected in series. These modifications are considered to be within skill of those in the art and within the spirit and scope of the claims. FIG. 1 shows an example of how to obtain two reaction chambers in one plasma reactor where the side chamber has a lower temperature than the main chamber, such that the first step as defined above is performed in the side chamber and the second step is performed in the main chamber before the product is taken out through the outlet at the bottom of the reactor.
  • Energy is supplied from the plasma are to heat the plasma gas. Some of the energy from the arc will be used to heat the surrounding reactor walls as well as the plasma generator itself. The resulting energy content of the plasma gas (the plasma gas enthalpy) is sufficient to evaporate the hydrocarbons. The hydrocarbons start a cracking and polymerization process, which results in the formation of polycycfic aromatic hydrocarbons (PAHs). The PAHs are the basis of graphitic sheets forming the micro-domains. The plasma gas enthalpy is kept at such a level that the main fraction of the gaseous hydrocarbons does not reach pyrolysis temperatures at the specified feed rate and residence time used. However, a small fraction of the feedstock will inevitably achieve sufficient energy during the residence time in the reactor to reach pyrolysis temperature and is consequently converted to conventional carbon black. This fraction should be kept as low as possible.
  • The PAHs leaves the reactor along with the plasma gas and is once more introduced in the reactor as a part of the plasma gas. The plasma gas enters the energy intensive plasma arc zone, wherein the PAHs during a fraction of a second are converted to graphitic micro-domains.
  • The feedstock feed rate for optimizing on graphitic micro-domain materials is in the range of 50-150 kg/h in a reactor employed by the inventor, but is not limited by this range. Both lower and higher feedstock feed rates might be used. The yield of the graphitic micro-domain material is better than 90% under optimal conditions. At least 10 percent of these domains have total disclinations larger than 60″. Taken into account the feedstock feed rate utilized, industrial amounts of micro-domain carbon material is achieved. By further up-scaling this will result in a price which is on the same level as commercial carbon black per unit weight of the material.
  • FIG. 1 shows a schematic drawing of the reactor. Further details concerning the reactor and the surrounding equipment are described in the applicant's Norwegian patent NO. 176511.
  • FIG. 2 shows a typical example of the content of the micro-domain material. Each piece in the sample forms a single graphitic domain and the alignment of the sheets in each domain is typically turbostratic, as determined from electron microscopy. The diameter of the domains is typically less than 5 micrometers and the thickness less than 100 nanometers. If a cone is made up of an uninterrupted sheet of graphite, except at the open edge, the only five possible types are possible due to the symmetry of graphite. These correspond to a total disclination of 60°, 120°, 180°, 240° and 300°. A total disclination of 0° corresponds to a flat domain. FIG. 3 shows schematically the projected angles of these structures. Examples of each of these types of domains are shown in FIGS. 4A, 4B, 4C, 4D and 4E. It is important to notice that all the cones are closed in the apex. The conical domains represent at least 10% of the material. The material of this invention consist of micro-domains of graphite of well-defined total disclinations TD (curvature), which have discrete values given by the formula

  • TD=N×60 degrees, where N=0, 1, 2, 3, 4 or 5,
  • and corresponds to the effective number of pentagons necessary to produce the particular total disclination.
  • The results the process is based on indicate that the total disclination nearly always is determined in the nucleation stage. It is earlier found that the probability of forming pentagons in the seed depends on the temperature (M. Endo and H. W. Kroto, J. Phys. Chem. 96, p. 6941, 1992). Hence, by varying the process parameters, the number of pentagons in the seed may increase, resulting in formation on nanotubes or closed shells.
  • The small size of the domains and the presence of various disclinations in the graphitic material produced in the present invention are useful for the incorporation of guest elements and compounds. The space between the domains will provide micro-pores for the flow of guest material so that it can reach each domain. The small size of the domains will allow rapid diffusion of guest material in and out of each layer composing them.
  • The invention will be illustrated in more detail with reference to the following examples, which should not be construed to be limiting in scope of the present invention. In Example I, the process parameters are chosen in such a way that conventional carbon black is formed at the first (and only) cycle of hydrocarbons through the reactor. By varying the feedstock feed rate, the plasma gas enthalpy and the residence time, it is shown in Example 2 that at the second cycle through the reactor, micro-domain graphitic materials can be produced from PAHs formed in the first cycle.
  • Example 1
  • Heavy fuel oil was heated to 1600° C. and introduced in the reactor by use of the self-invented axial aligned nozzle at a feed rate of 67 kg per hour. The reactor pressure was kept at 2 bar. Hydrogen was employed as plasma gas, and the plasma gas feed rate was 350 Nm3/h, while the gross power supply from the plasma generator was 620 kW. This resulted in a plasma gas enthalpy of 1.8 kWh/Nm3 H2. The time elapsed from the atomized oil was introduced until the product left the reactor was approximately 0.23 seconds.
  • The resulting carbon black was traditional amorphous of N-7xx quality. The volatile content of the carbon black was measured to 0.6%.
  • Example 2
  • In this example the oil feed rate, the hydrogen plasma gas enthalpy as well as the residence time was tuned in such a direction that the evaporated hydrocarbons did not achieve pyrolysis temperature during the first cycle. The residence time of the hydrocarbons during the first cycle through the reactor was minimized by increasing the oil and plasma gas feed rate.
  • Heavy fuel oil was heated to 160° C. and introduced in the reactor by use of the self-invented axial aligned nozzle at a feed rate of 115 kg per hour. The reactor pressure was kept at 2 bar. The hydrogen plasma gas feed rate was 450 Nm3/h, while the gross power of supply from the plasma generator was 1005 kW. This resulted in plasma gas enthalpy of 2.2 kWh/Nm3H2. The time elapsed from the oil was introduced until the PAHs left the reactor was approximately 0.16 seconds.
  • The resulting PAHs were reintroduced into the reactor in the plasma-are zone to produce a micro-domain graphitic material, with a yield higher than 90%. The volatile content of the carbon material was measured to 0.7%. All other process parameters were the same as for the first cycle.
  • Although in the example of the method has been described as a conversion of heavy oil to a micro-domain graphitic material, it should be understood that the method can be applied for all hydrocarbons, both liquid and gaseous. Also, the method may be performed as a batch or continuous production, with one or more plasma reactors in series etc. In the case where the PAHs formed in the first decomposition step is reintroduced into the same plasma reactor, the micro-domain graphitic materials formed in the second decomposition step are of course separated from the PAHs by any conventional suited means. This may be by filtering, cyclones etc.
  • Further, any gas that is inert and do not pollute the micro-domain graphitic products may be used as plasma gas, but hydrogen is specially suited since this element is present in the feedstock. The plasma gas may be recycled back into the reactor, if desired. It is also possible to employ the present method by introducing additional hydrocarbons through inlets at the sides of the decomposition reactor to control the temperature in the decomposition zone and/or to increase the yield, see the applicant's Norwegian patent NO. 176522.

Claims (5)

1-13. (canceled)
14. A carbon material comprising micro-domain graphitic materials comprising open carbon micro-cones with total disclination of 60° corresponding to cone angles of 112.9°.
15. A carbon material comprising micro-domain graphitic materials comprising open carbon micro-cones with total disclination of 120° corresponding to cone angles of 83.6°.
16. A carbon material comprising micro-domain graphitic materials comprising open carbon micro-cones with total disclination of 600 and 120°.
17. A carbon material comprising micro-domain graphitic materials comprising open carbon micro-cones with total disclination degrees 60° and/or 120°, corresponding to cone angles of respectively 112.9° and/or 83.6°.
US12/266,577 1997-03-25 2008-11-07 Micro-domain graphitic materials and method for producing same Abandoned US20090285747A1 (en)