JPH11114934A - Production of brick-tone tile - Google Patents

Production of brick-tone tile

Info

Publication number
JPH11114934A
JPH11114934A JP28577097A JP28577097A JPH11114934A JP H11114934 A JPH11114934 A JP H11114934A JP 28577097 A JP28577097 A JP 28577097A JP 28577097 A JP28577097 A JP 28577097A JP H11114934 A JPH11114934 A JP H11114934A
Authority
JP
Japan
Prior art keywords
tile
mold
brick
elastic body
periphery
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP28577097A
Other languages
Japanese (ja)
Other versions
JP3976378B2 (en
Inventor
Hiroaki Naito
博昭 内藤
Masayasu Kondo
正保 近藤
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Inax Corp
Original Assignee
Inax Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Inax Corp filed Critical Inax Corp
Priority to JP28577097A priority Critical patent/JP3976378B2/en
Publication of JPH11114934A publication Critical patent/JPH11114934A/en
Application granted granted Critical
Publication of JP3976378B2 publication Critical patent/JP3976378B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

PROBLEM TO BE SOLVED: To produce a tile inexpensively by collapsing its periphery so that it looks like a rough brick. SOLUTION: A tile raw material 6 is press-molded with the use of a form 1, an upper mold 3, and a lower mold 2, and the molded tile 7 is demolded and pressed again to collapse its periphery. Or, an elastomer 5 is stuck on the surface of the upper mold 3 and/or ht e lower mold 2. A protruded fringe part 5a is formed on the periphery of the elastomer 5 to enclose the raw material 6 in press molding so that the periphery of the molded tile is collapsed at demolding.

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【発明の属する技術分野】本発明は、乾式プレス成形に
より、成形したタイルの周囲が不規則に崩落したレンガ
調のタイルを製造するための技術に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a technique for producing a brick-like tile in which the periphery of a formed tile is irregularly collapsed by dry press molding.

【0002】[0002]

【従来の技術】近年店舗や住宅の外装における外壁の表
面は、自然な雰囲気が得られ、独自な趣が得られ、適度
なバラツキがある、割石状や岩肌状やレンガ調にするこ
とが好まれるようになってきている。そこで、特に、外
表面がレンガで施工したように見せるために、コンクリ
ートに着色剤を混ぜて薄板上に成形して乾燥し、コスト
を抑えたレンガ調のコンクリート板を得て、このレンガ
調コンクリート板を外壁に張り付けるようにした技術が
公知となっている。
2. Description of the Related Art In recent years, it is preferable that the surface of the outer wall of the exterior of a store or a house has a natural atmosphere, a unique taste, a moderate variation, a broken stone shape, a rock surface shape, and a brick tone. It is becoming more and more. Therefore, in order to make it look as if the outer surface was made of brick, concrete was mixed with a coloring agent, formed into a thin plate and dried to obtain a brick-like concrete plate with reduced cost. A technique for attaching a plate to an outer wall is known.

【0003】[0003]

【発明が解決しようとする課題】しかし、コンクリート
の薄板でレンガ調に構成すると、コンクリートは耐候性
が劣り、特に、凍結に弱いために、外装にレンガ調コン
クリートを使用すると、ヒビが入ったり、欠けたりし
て、外観を損ねてしまい、このヒビが入ったり、欠けた
部分を交換するのは大変面倒な作業となっていたのであ
る。そこで本発明はタイルをラフレンガ調のように見せ
たいために周囲を崩落させて、安価に製造できるように
しようとする。
However, when a brick-like concrete is used to form a brick-like concrete, the concrete has poor weather resistance, and is particularly vulnerable to freezing. It was chipped and spoiled the appearance, and replacing this cracked or missing part was a very laborious task. Therefore, in the present invention, in order to make the tile look like a rough brick, the surroundings are collapsed so that the tile can be manufactured at low cost.

【0004】[0004]

【課題を解決するための手段】本発明の解決しようとす
る課題は以上の如くであり、次に該課題を解決する為の
手段を説明する。即ち、枠型と上型と下型によりタイル
原料をプレス成形し、プレス成形した後のタイル成形体
を枠型より取り出し、該タイル成形体を再加圧してその
周囲を崩落させるようにしてレンガ調タイルを製造した
ものである。
The problem to be solved by the present invention is as described above. Next, means for solving the problem will be described. That is, the tile material is press-molded by the frame mold, the upper mold and the lower mold, the tile molded body after the press molding is taken out from the frame mold, and the tile molded body is repressurized so that the periphery thereof is collapsed so that the bricks are collapsed. It is made of toned tile.

【0005】または、上型、または、下型、または、上
型と下型の両方の表面に弾性体を貼設し、該弾性体の周
囲に凸縁部を形成して、プレス成形時にタイル原料の周
囲を囲み、離型時にタイル成形体の周囲を崩落させるよ
うにし、前記弾性体をラバーとし、65〜85度の硬度
としてレンガ調タイルを製造したものである。
[0005] Alternatively, an elastic body is stuck on the surface of the upper mold, the lower mold, or both the upper mold and the lower mold, and a convex edge is formed around the elastic body, and the tile is formed at the time of press molding. A brick-like tile is manufactured by surrounding the raw material and causing the periphery of the tile molded body to collapse at the time of mold release, using the elastic body as rubber, and setting the hardness to 65 to 85 degrees.

【0006】[0006]

【発明の実施の形態】次に本発明の実施例を説明する。
図1は本発明の再加圧によりレンガ調タイルを製造する
工程の一部を示すタイル成形型の断面図、図2は同じく
枠型を下げて再加圧の工程を示す断面図、図3は本発明
の弾性体を用いてレンガ調タイルを製造する工程の一部
を示すタイル成形型の断面図、図4は同じく圧力を解除
する工程を示す拡大断面図である。
Next, embodiments of the present invention will be described.
FIG. 1 is a cross-sectional view of a tile forming die showing a part of a process of manufacturing a brick tile by re-pressing according to the present invention. FIG. 2 is a cross-sectional view showing a process of lowering the frame die and re-pressing. Is a sectional view of a tile forming die showing a part of a step of manufacturing a brick tile using the elastic body of the present invention, and FIG. 4 is an enlarged sectional view showing a step of releasing pressure similarly.

【0007】レンガ調タイルの製造方法にはプレス成形
した後に取り出して再加圧する方法と、成形空間の周囲
にラバーを配置してプレス成形する二つの方法がある。
まず、図1、図2において再加圧する方法から説明す
る。1は枠型であり、該枠型1内に平面視長方形状の成
形空間4が形成され、該成形空間4内に金属より構成さ
れる下型2の表側が挿入されて、この成形空間4内にタ
イル原料6が充填される。該成形空間4上方に上型3が
配置されている。
[0007] There are two methods of manufacturing brick-like tiles: a method of taking out after press molding and re-pressing, and a method of arranging rubber around the molding space and press molding.
First, the method of re-pressurizing will be described with reference to FIGS. Reference numeral 1 denotes a frame mold, in which a rectangular molding space 4 in a plan view is formed, and the front side of a lower mold 2 made of metal is inserted into the molding space 4 to form the molding space 4. Is filled with a tile material 6. The upper die 3 is arranged above the molding space 4.

【0008】これら枠型1、下型2、上型3はそれぞれ
図示しない昇降機構によって昇降可能に構成され、それ
ぞれの駆動は制御装置によって制御されている。なお、
前記枠型1、下型2及び上型3は金属より構成され、該
下型2または上型3またはその両方の表面には、凹凸模
様や裏足等を成形するためにラバーを貼設する場合もあ
る。
The frame mold 1, the lower mold 2, and the upper mold 3 can be moved up and down by an elevating mechanism (not shown), and their driving is controlled by a controller. In addition,
The frame mold 1, the lower mold 2 and the upper mold 3 are made of metal, and rubber is attached to the surface of the lower mold 2 and / or the upper mold 3 or both to form a concavo-convex pattern or soles. In some cases.

【0009】このような成形型により本発明のレンガ調
タイルを製造するには、図1に示すように、従来のタイ
ルを製造する方法と同様に、まず、図1(a)のよう
に、前記成形空間4内にタイル原料6を充填して、図1
(b)のように、前記上型3を下降させることによっ
て、タイル原料6を加圧し成形してタイル成形体7を得
る。このときの加圧力は本実施例の場合約200kgf/cm
2 程度である。次に、図1(c)のように、タイル成形
体7が崩れたり、割れたりしないように、タイル成形体
7に掛かる圧力を開放しながら、下型2と上型3の両方
を上昇させる。このとき下型2と上型3の間でタイル成
形体7とは略接した状態としている。なお、上型と下型
で略接した状態で枠型を下げる場合もある。
In order to manufacture the brick-like tile of the present invention by using such a mold, as shown in FIG. 1, first, as shown in FIG. Filling the molding space 4 with the tile material 6, FIG.
As shown in (b), by lowering the upper die 3, the tile raw material 6 is pressed and molded to obtain a tile molded body 7. The pressing force at this time is approximately 200 kgf / cm in the case of this embodiment.
About 2 . Next, as shown in FIG. 1C, both the lower mold 2 and the upper mold 3 are raised while releasing the pressure applied to the tile molded body 7 so that the tile molded body 7 does not collapse or break. . At this time, the tile mold 7 is substantially in contact with the lower mold 2 and the upper mold 3. In some cases, the frame mold is lowered in a state where the upper mold and the lower mold are substantially in contact with each other.

【0010】次に、図2(a)のように、枠型1を下降
し、該枠型1の上面と下型2の上面が略一致するまで下
降する。そして、このタイル成形体の周囲が開放された
状態から上型3を下降させて再び弱い力、つまり、成形
時の加圧力よりもごく弱い力で加圧すると、タイル成形
体の周囲が崩れて、不規則に崩れた側面が得られるので
ある。なお、この再加圧力は本実施例では約5〜10kg
f/cm2 としている。
Next, as shown in FIG. 2A, the frame die 1 is lowered, and is lowered until the upper surface of the frame die 1 and the upper surface of the lower die 2 substantially coincide with each other. Then, when the upper mold 3 is lowered from the state where the periphery of the tile molded body is opened and pressed again with a weak force, that is, a force very small than the pressing force at the time of molding, the periphery of the tile molded body collapses. The result is an irregularly collapsed aspect. In this embodiment, the re-pressing force is about 5 to 10 kg.
f / cm 2 .

【0011】そして、上型3を上昇させて、このように
して得られたタイル成形体7は次の施釉または焼成工程
へ払い出され、周囲に崩れ落ちた崩落物7aは取り除か
れて、枠型1、下型2、上型3を初期状態に戻し、前記
と同じ作業を繰り返してレンガ調タイルの成形体7が得
るのである。
Then, the upper mold 3 is raised, and the tile molded body 7 thus obtained is discharged to the next glaze or firing step, and the collapsed material 7a that has collapsed around is removed, and the frame mold 7 is removed. 1, the lower mold 2 and the upper mold 3 are returned to the initial state, and the same operation as described above is repeated to obtain the brick-like tile molded body 7.

【0012】次に、成形空間の周囲に弾性体5を配置し
てプレス成形してレンガ調タイルを製造する方法を説明
する。図3に示すように、下型2と上型3の表面(成形
空間側)にラバー等よりなる弾性体5が貼設されてい
る。該弾性体5は中央部は薄くその表面にはレンガの表
面または割石状の表面の如くに転写できる凹凸が形成さ
れている。そして、弾性体5の周囲はタイル成形体7の
周囲を取り囲むように厚肉または盛り上げて凸縁部5a
を形成している。その表面も前記中央部と同様にレンガ
の表面または割石状の表面の如くに転写できる凹凸が形
成されている。この弾性体5の硬度は約65〜85度で
あり、従来から使用されている裏足用のラバーは90〜
100度としている。この弾性体5の硬さをこれ以下と
すると、軟らかすぎてタイルを成形することができず、
弾性体5はつぶれたり、破れたりする。硬過ぎると後述
する圧縮と膨張が得られず崩落が得られず、また、型か
ら脱型できないのである。
Next, a method for manufacturing a brick tile by press-forming the elastic body 5 around the forming space will be described. As shown in FIG. 3, an elastic body 5 made of rubber or the like is attached to the surface (molding space side) of the lower mold 2 and the upper mold 3. The elastic body 5 has a thin central portion, and has irregularities on its surface which can be transferred like a brick surface or a broken stone surface. Then, the periphery of the elastic body 5 is thickened or raised so as to surround the periphery of the tile molded body 7, and the convex edge portion 5a is formed.
Is formed. The surface is also formed with irregularities that can be transferred like a brick surface or a broken stone surface like the central portion. The hardness of the elastic body 5 is about 65 to 85 degrees, and the conventionally used rubber for soles is 90 to 85 degrees.
100 degrees. If the hardness of the elastic body 5 is less than this, it is too soft to form a tile,
The elastic body 5 is crushed or torn. If it is too hard, compression and expansion described below cannot be obtained, no collapse can be obtained, and the mold cannot be released from the mold.

【0013】このように構成した成形型によって、本発
明のレンガ調タイルの製造方法を説明する。図3(a)
に示すように、先ず、下型2と上型3にそれぞれ弾性体
5を貼設して、前記と同様に、枠型1の弾性体5と下型
2の弾性体5によって形成される成形空間4内にタイル
原料6が充填される。次に、図3(b)に示すように、
上型3を下降させて下型2との間のタイル原料6をプレ
ス成形する。このとき弾性体5も圧縮され、特に、周囲
の厚い部分である凸縁部5aに圧力が溜められる。そし
て、図4(a)に示すように、タイル成形体7に掛かる
圧力を開放しながら、下型2と上型3の両方を上昇させ
る(共上げ)。このとき弾性体5は上下方向に膨張す
る。この膨張によって膨張率の大きいタイル成形体7の
周囲は弾性体5の凸縁部5aによってズレが生じてタイ
ル成形体7の側面の一部を崩す。
The method of manufacturing the brick-like tile of the present invention using the thus-configured mold will be described. FIG. 3 (a)
As shown in (1), first, elastic bodies 5 are attached to the lower mold 2 and the upper mold 3, respectively, and the molding formed by the elastic body 5 of the frame mold 1 and the elastic body 5 of the lower mold 2 in the same manner as described above. The space 4 is filled with the tile raw material 6. Next, as shown in FIG.
The upper mold 3 is lowered to press-form the tile material 6 between the upper mold 3 and the lower mold 2. At this time, the elastic body 5 is also compressed, and pressure is accumulated particularly in the peripheral edge portion 5a which is a thick portion around the elastic body 5. Then, as shown in FIG. 4A, both the lower mold 2 and the upper mold 3 are raised while releasing the pressure applied to the tile molding 7 (co-raising). At this time, the elastic body 5 expands vertically. Due to this expansion, the periphery of the tile molded body 7 having a large expansion coefficient is displaced by the convex edge portion 5a of the elastic body 5, and a part of the side surface of the tile molded body 7 is broken.

【0014】次に、図4(b)に示すように、前記状態
から枠型1を下降させると、タイル成形体7側面に位置
する弾性体5の凸縁部5aが枠型1より露出して、加圧
成形によって弾性体5に蓄積された力が開放されて、弾
性体5は膨張して、凸縁部5bは側方へ広がる。一方、
この弾性体5の横方向への広がりによってタイル成形体
7の側面が崩落する。そして、この状態から上型3を上
昇させると、図4(c)に示すように、上下に弾性体5
・5が離れて元の状態に戻り、崩された崩落物7aは周
囲に落ちる。この崩れ落ちた崩落物7aの量や大きさは
タイル自体の成分が同一ではなく、均一でもないので、
タイル個々によって異なり、側面形状も不規則となり、
適度にバラツクようになるのである。そして、この側面
が崩れ落ちたタイル成形体は次の工程に送られるのであ
る。
Next, as shown in FIG. 4B, when the frame die 1 is lowered from the above state, the protruding edge portion 5a of the elastic body 5 located on the side surface of the tile molded body 7 is exposed from the frame die 1. Then, the force accumulated in the elastic body 5 by the pressure molding is released, the elastic body 5 expands, and the protruding edge portion 5b spreads to the side. on the other hand,
The lateral surface of the elastic body 5 causes the side surface of the tile molded body 7 to collapse. Then, when the upper die 3 is raised from this state, as shown in FIG.
5 is separated and returns to the original state, and the collapsed collapsed object 7a falls to the surroundings. Since the amount and size of the collapsed fallen object 7a are not the same and the components of the tile itself are not uniform,
Depending on each tile, the side shape is also irregular,
It becomes moderately variable. Then, the tile molded body whose side has collapsed is sent to the next step.

【0015】但し、本実施例では下型2と上型3の両方
に弾性体5・5を貼設しているが、下型2の表面のみ、
または上型3の表面のみに弾性体5を貼設して、該弾性
体5の周囲に構成した凸縁部5aの高さはタイルの厚さ
と略同じとなるようにし、タイル成形体7の周囲を囲め
るようにする。
However, in this embodiment, the elastic members 5 are attached to both the lower mold 2 and the upper mold 3.
Alternatively, the elastic body 5 is attached only to the surface of the upper die 3 so that the height of the protruding edge portion 5a formed around the elastic body 5 is substantially the same as the thickness of the tile. Be able to surround it.

【0016】[0016]

【発明の効果】本発明は以上の如く構成したので、次の
ような効果を奏するのである。即ち、請求項1の如く、
枠型と上型と下型によりタイル原料をプレス成形し、プ
レス成形した後のタイル成形体を枠型より取り出し、該
タイル成形体を再加圧してその周囲を崩落させるように
したので、プレス成形を行う上型(または下型でも可
能)の昇降制御プログラムを変更するだけで、その他の
製造のための部品を付加したり、原料に他の物質を混ぜ
たり、後工程で加工を加えたりすることなく、周囲が不
均一に崩落したレンガ調タイルが得られるようになった
のである。
As described above, the present invention has the following advantages. That is, as in claim 1,
The tile raw material was press-molded by the frame mold, the upper mold and the lower mold, and the tile molded body after the press molding was taken out of the frame mold, and the tile molded body was re-pressed so that the periphery thereof collapsed. By simply changing the elevation control program of the upper mold (or lower mold) that performs molding, it is possible to add other parts for manufacturing, mix other substances with raw materials, add processing in the post-process, etc. Without this, brick-like tiles with unevenly collapsed surroundings can be obtained.

【0017】または、請求項2の如く、上型、または、
下型、または、上型と下型の両方の表面に弾性体を貼設
し、該弾性体の周囲に凸縁部を形成して、プレス成形時
にタイル原料の周囲を囲み、離型時にタイル成形体の周
囲を崩落させるようにしたので、加圧時に弾性体が圧縮
され、離型時に弾性体が膨張してタイル成形体の周囲を
崩落させるようになり、タイル原料の成分は均一でない
ため、前記崩落も均一ではなく、タイル全てにおいてバ
ラツいて、後工程で加工を加えることなく、レンガ調タ
イルが得られるようになったのである。
Alternatively, as in claim 2, the upper mold or
An elastic body is attached to the surface of both the lower mold or the upper mold and the lower mold, and a convex edge is formed around the elastic body to surround the periphery of the tile material at the time of press molding, and to release the tile at the time of mold release. Since the periphery of the molded body is collapsed, the elastic body is compressed when pressurized, and the elastic body expands at the time of mold release and collapses around the tile molded body, and the components of the tile raw material are not uniform, In addition, the above-mentioned collapse is not uniform, and varies in all the tiles, so that brick-like tiles can be obtained without any processing in a later step.

【0018】また、請求項3の如く、前記弾性体をラバ
ーとし、65〜85度の硬度としたので、これ以上硬く
すると変形が小さく圧力を蓄えることができず、崩落を
生じさせることができず、また、これ以上軟らかくする
と、成形型として必要な硬さが得られず、弾性体がつぶ
れたり、破れたりし、または、流動してタイル成形体が
歪んだ形となったりする。従って、65〜85度の硬度
とすることによって、タイルは従来と同様に得られ、周
囲のみ崩落したバラツキのあるタイルが得られるように
なったのである。
Further, since the elastic body is made of rubber and has a hardness of 65 to 85 degrees as described above, if it is harder than this, deformation is small and pressure cannot be stored, and collapse can occur. If it is softer than this, the required hardness of the mold will not be obtained, and the elastic body will be crushed or torn, or it will flow and the tile molded body will be distorted. Therefore, by setting the hardness to 65 to 85 degrees, the tile can be obtained in the same manner as in the related art, and a tile having a variation in which only the periphery has collapsed can be obtained.

【図面の簡単な説明】[Brief description of the drawings]

【図1】本発明の再加圧によりレンガ調タイルを製造す
る工程の一部を示すタイル成形型の断面図である。
FIG. 1 is a cross-sectional view of a tile mold showing a part of a process of manufacturing a brick tile by re-pressing according to the present invention.

【図2】同じく枠型を下げて再加圧の工程を示す断面図
である。
FIG. 2 is a cross-sectional view showing a step of lowering the frame mold and repressurizing the same.

【図3】本発明の弾性体を用いてレンガ調タイルを製造
する工程の一部を示すタイル成形型の断面図である。
FIG. 3 is a sectional view of a tile mold showing a part of a process of manufacturing a brick tile using the elastic body of the present invention.

【図4】同じく圧力を解除する工程を示す拡大断面図で
ある。
FIG. 4 is an enlarged sectional view showing a step of releasing pressure similarly.

【符号の説明】[Explanation of symbols]

2 下型 3 上型 5 弾性体 5a 凸縁部 7 タイル成形体 2 Lower mold 3 Upper mold 5 Elastic body 5a Convex edge 7 Tile molding

Claims (3)

【特許請求の範囲】[Claims] 【請求項1】 枠型と上型と下型によりタイル原料をプ
レス成形し、プレス成形した後のタイル成形体を枠型よ
り取り出し、該タイル成形体を再加圧してその周囲を崩
落させることを特徴とするレンガ調タイルの製造方法。
1. Tile raw material is press-molded by a frame mold, an upper mold and a lower mold, a tile molded body after the press molding is taken out from the frame mold, and the tile molded body is repressurized to collapse its periphery. A method for producing a brick tile.
【請求項2】 上型、または、下型、または、上型と下
型の両方の表面に弾性体を貼設し、該弾性体の周囲に凸
縁部を形成して、プレス成形時にタイル原料の周囲を囲
み、離型時にタイル成形体の周囲を崩落させるようにし
たことを特徴とするレンガ調タイルの製造方法。
2. An elastic body is stuck on the surface of an upper mold, a lower mold, or both of an upper mold and a lower mold, and a convex edge is formed around the elastic body, and the tile is formed at the time of press molding. A method of manufacturing a brick-like tile, wherein a periphery of a raw material is surrounded, and the periphery of a tile molded body is collapsed at the time of mold release.
【請求項3】 前記弾性体をラバーとし、65〜85度
の硬度としたことを特徴とする請求項2記載のレンガ調
タイルの製造方法。
3. The method for manufacturing a brick-like tile according to claim 2, wherein the elastic body is made of rubber and has a hardness of 65 to 85 degrees.
JP28577097A 1997-10-17 1997-10-17 Brick tone tile manufacturing method Expired - Fee Related JP3976378B2 (en)