JPH06286363A - Invisible information record medium and information recording method which handles it - Google Patents

Invisible information record medium and information recording method which handles it

Info

Publication number
JPH06286363A
JPH06286363A JP5076723A JP7672393A JPH06286363A JP H06286363 A JPH06286363 A JP H06286363A JP 5076723 A JP5076723 A JP 5076723A JP 7672393 A JP7672393 A JP 7672393A JP H06286363 A JPH06286363 A JP H06286363A
Authority
JP
Japan
Prior art keywords
infrared
layer
information recording
recording medium
invisible information
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP5076723A
Other languages
Japanese (ja)
Other versions
JP3326859B2 (en
Inventor
Yoshie Arai
美江 新井
Noriyuki Ito
則之 伊藤
Osahisa Matsudaira
長久 松平
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toppan Inc
Original Assignee
Toppan Printing Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toppan Printing Co Ltd filed Critical Toppan Printing Co Ltd
Priority to JP07672393A priority Critical patent/JP3326859B2/en
Publication of JPH06286363A publication Critical patent/JPH06286363A/en
Application granted granted Critical
Publication of JP3326859B2 publication Critical patent/JP3326859B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

PURPOSE:To provide an invisible information record medium with which invisible information can be recorded, recorded information can be concealed without unnatural feeling, information is recorded in a thermal recording layer as an intermediate layer of the invisible information record medium by laser beam, and alteration of the record by a thermal head is impossible and forgery of the record can be prevented, and the surface shape does not change. CONSTITUTION:On a surface of a base material 1, an infrared ray absorbing ink layer 2 which has, for example, diphosphorus pentoxide as a main component and is made of phosphoric acid white crystal powder containing Fe<2+> and/or Cu<2+>, and a thermal recording layer 3 which is made of, for example, hollow microcapsule and has the same color as the infrared ray absorbing ink layer 2 and scatters the infrared rays at room temperature and increases its infrared ray transmission factor at heating with a heat higher than a predetermined temperature are layered. The base material 1 is further covered with a protective layer 4 made of infrared ray transmitting material.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は、不可視な可変情報を記
録することが可能な不可視情報記録媒体と、それを取り
扱う情報記録方法に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to an invisible information recording medium capable of recording invisible variable information and an information recording method for handling the invisible information recording medium.

【0002】[0002]

【従来の技術】赤外吸収材料を利用した不可視情報記録
媒体は従来から各種提案されており、一部に利用されて
いる。
2. Description of the Related Art Various types of invisible information recording media using infrared absorbing materials have been proposed and some of them have been used.

【0003】固定情報を記録する不可視情報記録媒体と
しては、カーボン等の有色である赤外吸収材料によって
バーコード等を印刷し、濃色の赤外透過材料を用いて隠
蔽層を設ける方法や、カーボン等の赤外線を吸収するイ
ンキで押印した後、黒色の赤外透過フィルムで隠蔽する
ものが実用、提案されている。
As an invisible information recording medium for recording fixed information, a method of printing a bar code or the like with a colored infrared absorbing material such as carbon and providing a concealing layer using a dark infrared transmitting material, It has been proposed and put into practical use that the material is imprinted with an ink that absorbs infrared rays, such as carbon, and then hidden with a black infrared transmission film.

【0004】また、可変情報を記録する不可視情報記録
媒体としては、発色部が可視及び赤外線を吸収する材料
を用いた記録層を有する媒体上に赤外透過材料からなる
隠蔽層を設けたものが実用化、提案されている。
As an invisible information recording medium for recording variable information, a medium having a recording layer made of a material whose coloring portion absorbs visible light and infrared light is provided with a concealing layer made of an infrared transmitting material. Practical application, proposed.

【0005】これらの隠蔽層は黒色である為、隠蔽され
た情報を直接見る事はできないが、隠蔽層を目視できる
ので、その下に情報が隠されている事は一目瞭然であ
り、偽造を試みる人間のターゲットになり易かった。
Since these hidden layers are black, the hidden information cannot be seen directly, but since the hidden layer can be seen, it is obvious that the information is hidden under the hidden layers, and forgery is tried. It was easy to become a human target.

【0006】他方、以上の可変情報を記録する不可視情
報記録媒体にあっては、サーマルヘッド等を用いた加熱
記録が必須であることから、記録時に表面形状が変化す
ることが避けられないので、記録され隠蔽された情報が
光の加減で見えてしまう。また、近年ではサーマルヘッ
ド等での熱による記録の変造が行われる等の問題点があ
った。
On the other hand, in the above invisible information recording medium for recording variable information, since heating recording using a thermal head or the like is essential, it is unavoidable that the surface shape changes during recording. The recorded and hidden information becomes visible under the control of light. Further, in recent years, there has been a problem that recording is altered by heat from a thermal head or the like.

【0007】更にまた、サーマルヘッドを用いた加熱記
録方法では、保護層を厚くすることも困難であるため、
膜強度の無い媒体になりがちであった。
Furthermore, in the heating recording method using a thermal head, it is difficult to thicken the protective layer,
It tended to be a medium without film strength.

【0008】[0008]

【発明が解決しようとする課題】本発明はこのような問
題点に着目してなされたもので、その課題とするところ
は、可変情報を記録でき、不自然さを感じさせずに記録
情報を隠蔽することができ、かつレーザービームにより
不可視情報記録媒体の中間層となる感熱記録層に記録し
て、サーマルヘッドでの記録の改ざんを不可能偽造防止
効果があり、また、表面形状が変化しない不可視情報記
録媒体及びそれを取り扱う情報記録方法を提供すること
にある。
SUMMARY OF THE INVENTION The present invention has been made in view of such a problem. The problem is that variable information can be recorded and recorded information can be recorded without feeling unnaturalness. It is possible to conceal, and it is impossible to falsify the recording by the thermal head by recording on the heat-sensitive recording layer which is the intermediate layer of the invisible information recording medium by the laser beam. An object is to provide an invisible information recording medium and an information recording method for handling the medium.

【0009】[0009]

【課題を解決するための手段】請求項1記載の発明は、
基材の表面に、赤外線吸収インキ層と、前記赤外線吸収
インキ層と同系色で、常温では赤外線を散乱し、所定の
温度以上の加熱で赤外線透過率が増大する感熱記録層を
積層し、更に前記感熱記録層を赤外透過材料から構成さ
れる保護層で覆ったことを特徴とする不可視情報記録媒
体である。
The invention according to claim 1 is
On the surface of the base material, an infrared absorbing ink layer and a thermosensitive recording layer having the same color as the infrared absorbing ink layer, which scatters infrared rays at room temperature and increases the infrared transmittance by heating at a predetermined temperature or more, are further laminated. The invisible information recording medium is characterized in that the heat-sensitive recording layer is covered with a protective layer made of an infrared transmitting material.

【0010】請求項2記載の発明は、基材の表面に、赤
外線吸収インキ層と、常温では赤外線を散乱し、所定の
温度以上の加熱で赤外線透過率が増大する感熱記録層を
積層し、前記赤外線吸収インキ層と同系色で赤外線透過
性のインキからなる隠蔽層で覆ったことを特徴とする不
可視情報記録媒体である。
According to a second aspect of the present invention, an infrared absorbing ink layer and a heat-sensitive recording layer that scatters infrared rays at room temperature and increases the infrared transmittance by heating above a predetermined temperature are laminated on the surface of a substrate. The invisible information recording medium is characterized in that it is covered with a concealing layer made of an infrared transmitting ink having a similar color to the infrared absorbing ink layer.

【0011】請求項3記載の発明は、請求項2記載の発
明を前提とし、更に前記隠蔽層を赤外透過材料から構成
される保護層で覆ったことを特徴とする不可視情報記録
媒体である。
The invention according to claim 3 is based on the invention according to claim 2, and is an invisible information recording medium characterized in that the concealing layer is covered with a protective layer made of an infrared transmitting material. .

【0012】請求項4記載の発明は、請求項1、2、3
記載の発明を前提とし、感熱記録層が本質的に中空マイ
クロカプセルから構成されることを特徴とする不可視情
報記録媒体である。
The invention according to claim 4 is the invention according to claims 1, 2, and 3.
Based on the described invention, the invisible information recording medium is characterized in that the heat-sensitive recording layer is essentially composed of hollow microcapsules.

【0013】請求項5記載の発明は、請求項1、2、3
記載の発明を前提とし、赤外線吸収インキ層が白色ある
いは淡色であることを特徴とする請求項1、2、3記載
の不可視情報記録媒体である。
The invention as claimed in claim 5 is as follows.
The invisible information recording medium according to any one of claims 1 to 3, characterized in that the infrared absorbing ink layer is white or light color based on the invention described above.

【0014】請求項6記載の発明は、請求項1、2、
3、5記載の発明を前提とし、赤外線インキ層中の赤外
吸収材料が五二酸化リンを主成分とし、Fe2+及び/ま
たはCu2+を含有するリン酸白色結晶粉末から構成され
ることを特徴とする請求項1、2、3、5記載の不可視
情報記録媒体である。
The invention according to claim 6 is the invention as defined in claims 1, 2 and
Based on the inventions 3 and 5, the infrared absorbing material in the infrared ink layer is composed of phosphoric acid white crystalline powder containing phosphorus pentoxide as a main component and Fe 2+ and / or Cu 2+. The invisible information recording medium according to claim 1, 2, 3, or 5.

【0015】請求項7記載の発明は、請求項1記載の不
可視情報記録媒体を取り扱う情報記録方法であって、前
記保護層側から赤外線を照射し、感熱記録層を加熱する
ことにより情報を記録することを特徴とする不可視情報
記録媒体の情報記録方法である。
The invention according to claim 7 is an information recording method for handling the invisible information recording medium according to claim 1, wherein information is recorded by irradiating infrared rays from the protective layer side and heating the heat-sensitive recording layer. An information recording method for an invisible information recording medium, characterized in that:

【0016】請求項8記載の発明は、請求項2、3記載
の不可視情報記録媒体を取り扱う情報記録方法であっ
て、前記隠蔽層側から赤外線を照射し、感熱記録層を加
熱することにより情報を記録することを特徴とする不可
視情報記録媒体の情報記録方法である。
The invention according to claim 8 is an information recording method for handling the invisible information recording medium according to claims 2 and 3, wherein information is obtained by irradiating infrared rays from the concealing layer side to heat the heat-sensitive recording layer. Is recorded on the invisible information recording medium.

【0017】請求項9記載の発明は、請求項7、8記載
の発明を前提とし、前記赤外線の照射による記録が赤外
線リーダー及び/または赤外スコープにより読み取り可
能なパターンであることを特徴とする不可視情報記録媒
体を取り扱う情報記録方法。である。
The invention described in claim 9 is based on the invention described in claims 7 and 8, characterized in that the recording by the irradiation of infrared rays is a pattern readable by an infrared reader and / or an infrared scope. Information recording method for handling invisible information recording medium. Is.

【0018】以下に、本発明に係わる不可視情報記録媒
体を図1及び図2を用いて説明する。
The invisible information recording medium according to the present invention will be described below with reference to FIGS. 1 and 2.

【0019】本発明に係わる基材(1)は、用途に応じ
て種々のものが使用できるが、例えば紙や、PET、塩
ビ等のプラスチック等が用いられる。尚、後述する各層
を基材上に部分的に設ける際はその色を合わせる必要が
ある。
Various materials can be used as the base material (1) according to the present invention depending on the application, and for example, paper, plastics such as PET, vinyl chloride and the like are used. When each layer described below is partially provided on the base material, it is necessary to match the colors.

【0020】本発明に係わる赤外吸収インキ層(2)
は、赤外線吸収インキをスクリーン印刷方法等の公知の
印刷方法により1μm〜10μmの膜厚で印刷して設け
る。ここで用いる赤外線吸収インキとは、通常のカーボ
ンブラック等を顔料とするインキでもよいが、前記イン
キは可視領域にも吸収があるため、情報が隠されている
事は一目瞭然となる虞がある。よって、赤外線吸収イン
キ層は白色あるいは淡色であることが好ましい。
Infrared absorbing ink layer (2) according to the present invention
Is provided by printing an infrared absorbing ink with a film thickness of 1 μm to 10 μm by a known printing method such as a screen printing method. The infrared absorbing ink used here may be an ink having a pigment such as ordinary carbon black, but since the ink also absorbs in the visible region, it may be obvious that information is hidden. Therefore, the infrared absorbing ink layer is preferably white or light colored.

【0021】ところで、前記赤外線吸収インキ層は、前
記したように白色あるいは淡色であることが好ましいの
で、白色あるいは淡色の赤外吸収材料を例示すると、F
2+及び/またはCu2+を含有するガラス系粉末、Fe
2+及び/またはCu2+を20重量%以上含み五二酸化リ
ン(P2 5 )を主成分とするとする結晶粉末、六塩化
タングステンとリン酸エステル及び/または亜リン酸と
の白色系反応生成物等の白色粉末、シアニン系、フタロ
シアニン系、ナフタロシアニン系、アントラキノン系、
アミニウム系、ジチオール金属錯塩系、ジインモニウム
系、トリフェニルメタン系、クロコニックメチン系、ア
ズレニオウム系、ピリリウム系等の赤外吸収性染料が挙
げられる
By the way, since the infrared absorbing ink layer is preferably white or light colored as described above, a white or light infrared absorbing material is exemplified by F.
Glass-based powder containing e 2+ and / or Cu 2+ , Fe
Crystal powder containing 20% by weight or more of 2+ and / or Cu 2+ and containing phosphorus pentaoxide (P 2 O 5 ) as a main component, white reaction of tungsten hexachloride with phosphoric acid ester and / or phosphorous acid White powder such as products, cyanine-based, phthalocyanine-based, naphthalocyanine-based, anthraquinone-based,
Infrared absorbing dyes such as aminium-based, dithiol metal complex-based, diimmonium-based, triphenylmethane-based, croconic methine-based, azulenium-based, and pyrylium-based

【0022】前記五二酸化リンを主成分とし、Fe2+
び/またはCu2+を含有するリン酸塩系白色結晶粉末を
より具体的に説明すると、五二酸化リンを重量%で40
〜70%、Fe2+及び/またはCu2+をそれぞれ30〜
70%含む結晶粉末である。このリン酸塩系白色結晶粉
末は前記の組成を有するリン酸塩系の組成物についてこ
れを融解し、かつ結晶化させてリン酸塩系白色結晶を求
めると共にこれを粉末化したものである。尚、このリン
酸塩系白色結晶粉末についても必要に応じて以下の化合
物を含有していてもよい。
More specifically, the phosphate-based white crystalline powder containing phosphorus pentoxide as the main component and containing Fe 2+ and / or Cu 2+ will be described in more detail.
~ 70%, Fe 2+ and / or Cu 2+ 30 ~, respectively
It is a crystal powder containing 70%. This phosphate-based white crystal powder is obtained by melting and crystallizing a phosphate-based composition having the above composition to obtain a phosphate-based white crystal, and powdering this. The phosphate-based white crystalline powder may also contain the following compounds, if necessary.

【0023】 Al2 3 2.0〜10.0重量% B2 3 1.0〜30.0重量% MgO 3.0〜10.0重量% ZnO 0〜3.0重量% K2 O 0〜15.0重量% BaO 0〜10.0重量% SrO 0〜1.0重量% Ni、Co、Se 微量Al 2 O 3 2.0 to 10.0% by weight B 2 O 3 1.0 to 30.0% by weight MgO 3.0 to 10.0% by weight ZnO 0 to 3.0% by weight K 2 O 0-15.0 wt% BaO 0-10.0 wt% SrO 0-1.0 wt% Ni, Co, Se Trace amount

【0024】また、前記Fe2+及び/またはCu2+を含
有するガラス系粉末材料をより具体的に説明すると、五
二酸化リン(P2 5 )を主成分とし、酸化鉄及び/ま
たは酸化銅を1.0重量%以上含む粉末材料で、よりこ
のましくは五二酸化リンを重量%で35.0〜80.0
%、酸化鉄及び酸化銅をそれぞれ0〜3.0%含むガラ
ス系粉末材料であることを特徴とする。尚、前記ガラス
系粉末材料内には必要に応じて以下の化合物を含有して
いてもよい。すなわち、
More specifically, the glass-based powder material containing Fe 2+ and / or Cu 2+ will be described in more detail. Phosphorus pentaoxide (P 2 O 5 ) is the main component, and iron oxide and / or oxide is used. A powder material containing 1.0 wt% or more of copper, more preferably 35.0 to 80.0 wt% of phosphorus pentoxide.
%, Iron oxide and copper oxide, each of which is a glass-based powder material containing 0 to 3.0%. The glass-based powder material may contain the following compounds, if necessary. That is,

【0025】 Al2 3 2.0〜10.0重量% B2 3 1.0〜30.0重量% MgO 3.0〜10.0重量% ZnO 0〜3.0重量% K2 O 0〜15.0重量% BaO 0〜10.0重量% SrO 0〜1.0重量% Ni、Co、Se 微量Al 2 O 3 2.0 to 10.0% by weight B 2 O 3 1.0 to 30.0% by weight MgO 3.0 to 10.0% by weight ZnO 0 to 3.0% by weight K 2 O 0-15.0 wt% BaO 0-10.0 wt% SrO 0-1.0 wt% Ni, Co, Se Trace amount

【0026】尚、白色度の点では、前記ガラス系粉末材
料及び白色結晶系粉末材料が良好であり、赤外線吸収能
の点では、白色結晶系粉末材料及び赤外吸収性染料が良
好である。
From the standpoint of whiteness, the glass-based powder material and the white crystalline powder material are good, and from the viewpoint of infrared absorbing ability, the white crystalline powder material and the infrared absorbing dye are good.

【0027】これらの顔料をインキ化するために用いる
バインダーとしては塩化ビニル―錯塩ビニル重合樹脂、
飽和ポリエステル樹脂、ポリウレタンエラストマー等が
用いられる。これらのバインダーは溶剤を除くインキ組
成分中に20重量%以上含まれる事が望ましい。
As a binder used for forming these pigments into ink, vinyl chloride-complex salt vinyl polymer resin,
Saturated polyester resin, polyurethane elastomer, etc. are used. These binders are preferably contained in the ink composition excluding the solvent in an amount of 20% by weight or more.

【0028】また、インキ化するために用いられる溶剤
としては、トルエン、メチルイソブチルケトン、キシレ
ン、シクロヘキサノール、酢酸イソブチル、シクロヘキ
サノン、メチルシクロヘキサノン、エチレングリコール
モノブチルエーテル等のグリコール誘導体等、またはこ
れらの混合溶媒が挙げられる。また、前記材料に加え消
泡剤、滑剤等を含むこともできる。
As the solvent used for forming an ink, toluene, methyl isobutyl ketone, xylene, cyclohexanol, isobutyl acetate, cyclohexanone, methylcyclohexanone, a glycol derivative such as ethylene glycol monobutyl ether, or a mixed solvent thereof is used. Is mentioned. Further, in addition to the above-mentioned materials, a defoaming agent, a lubricant and the like can be included.

【0029】前記のように構成された赤外線吸収インキ
層は、後述する上層の存在に係わらす、750、78
0、810、830、905nm等の赤外線(または赤
外スコープ)により黒色パターンとして識別できる。
The infrared absorbing ink layer having the above-mentioned structure is 750, 78 depending on the presence of the upper layer described later.
It can be identified as a black pattern by infrared rays (or infrared scope) of 0, 810, 830, 905 nm or the like.

【0030】本発明に係わる感熱記録層(3)は、常温
では赤外線を散乱し、所定の温度以上の加熱で赤外線透
過率が増大する層である。前記のような特性を示す記録
材料を例示すると、乳化重合法等で形成される粒径0.
05〜1μm程度の中空マイクロカプセルが挙げられ、
本質的に中空マイクロカプセルを乳化分散する事により
得たエマルジョンを赤外線吸収インキ層(2)上に塗布
乾燥することにより設けられる。
The heat-sensitive recording layer (3) according to the present invention is a layer which scatters infrared rays at room temperature and whose infrared transmittance increases by heating above a predetermined temperature. As an example of a recording material having the above-mentioned characteristics, a particle size of 0.
Hollow microcapsules of about 05 to 1 μm can be mentioned,
It is provided by coating and drying an emulsion obtained by essentially emulsifying and dispersing hollow microcapsules on the infrared absorbing ink layer (2).

【0031】かかる中空マイクロカプセルが乳化分散さ
れている感熱記録層は、常温では赤外線の入射に対し中
空マイクロカプセル内の空気の存在により光の屈折率の
変化が起こり、その結果、光の散乱(乱反射)が起こり
赤外線透過率が低下する。これに対し、所定以上の温
度、即ち中空マイクロカプセルを形成する樹脂のガラス
転移点以上に加熱する事によりマイクロカプセルの破
壊、融着が起こり、粒子−空気界面が減少し、光の散乱
が抑制され透明化し、赤外線の透過率が増大する。
In the heat-sensitive recording layer in which the hollow microcapsules are emulsified and dispersed, the refractive index of light changes due to the presence of air in the hollow microcapsules at room temperature due to the incidence of infrared rays, and as a result, the scattering of light ( Diffuse reflection occurs and the infrared transmittance decreases. On the other hand, by heating above a predetermined temperature, that is, above the glass transition point of the resin forming the hollow microcapsules, the microcapsules are destroyed and fused, the particle-air interface is reduced, and light scattering is suppressed. It becomes transparent and the infrared ray transmittance increases.

【0032】このようなマイクロカプセルを形成するた
めの壁材料としては、ガラス転移点温度が50℃〜15
0℃程度のものが好ましく、ポリユアレ、ポリエステ
ル、ポリカーボネート、尿素−ホルムアルデヒド樹脂、
メラミン樹脂、ポリスチレン、スチレンメタクリレート
共重合体、ゼラチン、ポリビニルピロリドン、ポリビニ
ルアルコール等が挙げられ所望の透明化温度に応じて選
択すれば良い。
The wall material for forming such microcapsules has a glass transition temperature of 50 ° C. to 15 ° C.
It is preferably about 0 ° C., and polyurea, polyester, polycarbonate, urea-formaldehyde resin,
Melamine resin, polystyrene, styrene-methacrylate copolymer, gelatin, polyvinylpyrrolidone, polyvinyl alcohol, etc. may be mentioned and may be selected according to the desired transparency temperature.

【0033】前記感熱記録層は、これらの乳化分散によ
り得られたエマルジョンとし、基材上の赤外線吸収イン
キ層上に、スクリーン印刷法、グラビア印刷法等の公知
の印刷方法で塗布乾燥することにより形成できる。尚、
本発明の感熱記録層は通常白色あるいは淡色であるが、
その下層の赤外線吸収インキ層は、組成により極薄い青
緑色を呈する場合があり、この上に感熱記録層を設け、
記録像を形成する(感熱記録層を透明化)と、下層の赤
外線吸収インキ層の極薄い青緑色が露出し、僅かなコン
トラストが生じ記録像が目視可能となる虞があるが、そ
の場合、感熱記録層に赤外線を透過する青緑色の染料ま
たは有色透明顔料を添加することにより、記録(情報)
が目視不可能となる。
The heat-sensitive recording layer is an emulsion obtained by emulsifying and dispersing these, and is coated and dried on the infrared absorbing ink layer on the substrate by a known printing method such as a screen printing method and a gravure printing method. Can be formed. still,
The heat-sensitive recording layer of the present invention is usually white or light color,
The underlying infrared absorbing ink layer may exhibit an extremely thin blue-green color depending on the composition, and a heat-sensitive recording layer may be provided on it.
When a recorded image is formed (the thermosensitive recording layer is made transparent), an extremely thin blue-green color of the lower infrared absorbing ink layer is exposed, and a slight contrast may occur, which may make the recorded image visible. Recording (information) by adding a blue-green dye or a colored transparent pigment that transmits infrared rays to the heat-sensitive recording layer
Becomes invisible.

【0034】よって、前記のように感熱記録層に赤外線
の照射により記録された部分は、後述する上層の保護層
の存在に係わらず、750、780、810、830、
905nmの赤外線(または赤外スコープ)により黒色
パターンとして識別され、非記録部分は白色として識別
できる。
Therefore, the portion recorded by the irradiation of infrared rays on the thermal recording layer as described above is 750, 780, 810, 830, regardless of the presence of the upper protective layer described later.
It can be identified as a black pattern by the infrared ray (or infrared scope) of 905 nm, and the non-recorded portion can be identified as white.

【0035】尚、前記感熱記録層の情報を記録した部分
は、バーコード、文字、数字、図柄等のパターンで設け
られても良い。その場合、公知の赤外線リーダーまたは
赤外スコープを用いてパターンを読み取り情報を再生す
る。
The portion of the heat-sensitive recording layer in which the information is recorded may be provided in a pattern such as a bar code, letters, numbers, and patterns. In that case, a known infrared reader or infrared scope is used to read the pattern and reproduce the information.

【0036】本発明に係わる隠蔽層(5)は隠蔽層を覆
うために、請求項2に記載の発明において任意に設けら
れる層であるが、前記赤外線吸収インキ層と同系色であ
り、赤外線透過性のインキを前記感熱記録層を覆うよう
に塗布形成して設けたものである。隠蔽層に用いること
のできるインキとしては、オフセット印刷等に用いられ
る、いわゆるプロセスインキが挙げられる。
The concealing layer (5) according to the present invention is a layer optionally provided in the invention according to claim 2 for covering the concealing layer, but it has the same color as the infrared absorbing ink layer and transmits infrared rays. Ink is applied and formed so as to cover the thermosensitive recording layer. Examples of the ink that can be used for the hiding layer include so-called process inks used for offset printing and the like.

【0037】本発明に係わる保護層(4)は隠蔽層ある
いは感熱記録層を覆うために、請求項1に記載の発明で
は必須、請求項2に記載の発明では任意に設けられる層
であるが、赤外透過材料からなり、記録時に表面形状が
変化が少ない特性を有するものである。尚、本発明に係
わる不可視情報記録媒体の情報記録方法として、レーザ
ービームによる赤外線による情報の記録方法をとれば、
赤外線の透過率が極端に悪化しない限り保護層を厚くす
ることが可能であるため、膜強度の強い媒体となる。
The protective layer (4) according to the present invention is a layer which is essential in the invention described in claim 1 and is optionally provided in the invention described in claim 2 in order to cover the concealing layer or the heat-sensitive recording layer. It is made of an infrared transmitting material and has a characteristic that the surface shape thereof is hardly changed during recording. As an information recording method for the invisible information recording medium according to the present invention, if an infrared information recording method using a laser beam is used,
Since the protective layer can be made thick unless the transmittance of infrared rays is extremely deteriorated, the medium has a strong film strength.

【0038】保護層を構成する材料を例示すると、ゼラ
チン、でんぷんのごとき天然高分子、硝酸繊維素、カル
ボキシメチルセルローズのごとき繊維素誘導体、塩化ゴ
ム、環化ゴムのごとき天然ゴム可塑物などの半合成高分
子物、ポリイソブチレン、ポリスチロール、テルペン樹
脂、ポリアクリル酸、ポリアクリル酸エステル、ポリメ
タアクリル酸エステル、ポリアクリルニトリル、ポリア
クリルアミド、ポリ酢酸ビニル、ポリビニルアルコー
ル、ポリビニルピロリドン、ポリアセタール樹脂、ポリ
塩化ビニル、ポリビニルピリジン、ポリビニルカルバゾ
ール、ポリブタジエン、ポリスチレン−ブタジエン、ブ
チルゴム、ポリオキシメチレン、ポリエチレンイミン、
ポリエチレンイミンハイドロクロライド、ポリ(2−ア
クリルオキシエチルジメチルスルホニウムクロライド)
などのごとき重合型合成高分子、フェノール樹脂、アミ
ノ樹脂、トルエン樹脂、アルキッド樹脂、不飽和ポリエ
ステル樹脂アリル樹脂、ポリカーボネート、ポリアマイ
ド樹脂、ポリエーテル樹脂、フラン樹脂、チオコールゴ
ムなどのごとき縮合重合型合成高分子、ポリウレタン、
ポリ尿素、エポキシ樹脂などのごとき付加重合型樹脂が
挙げられる。
Examples of materials constituting the protective layer include semi-polymers such as gelatin, natural polymers such as starch, fibrin nitrate, fibrin derivatives such as carboxymethyl cellulose, chlorinated rubber, and natural rubber plastics such as cyclized rubber. Synthetic polymer, polyisobutylene, polystyrene, terpene resin, polyacrylic acid, polyacrylic ester, polymethacrylic ester, polyacrylonitrile, polyacrylamide, polyvinyl acetate, polyvinyl alcohol, polyvinylpyrrolidone, polyacetal resin, poly Vinyl chloride, polyvinyl pyridine, polyvinyl carbazole, polybutadiene, polystyrene-butadiene, butyl rubber, polyoxymethylene, polyethylene imine,
Polyethyleneimine hydrochloride, poly (2-acryloxyethyl dimethylsulfonium chloride)
Polymerization type synthetic polymer such as phenol resin, amino resin, toluene resin, alkyd resin, unsaturated polyester resin allyl resin, polycarbonate, polyamide resin, polyether resin, furan resin, thiochol rubber, etc. , Polyurethane,
Examples thereof include addition polymerization type resins such as polyurea and epoxy resin.

【0039】[0039]

【作用】請求項1〜6記載の発明によれば、赤外線を照
射することで情報の書き込みができるので、可変情報を
記録でき、不自然さを感じさせずに記録情報を隠蔽する
ことができ、かつレーザービームにより媒体の中間層だ
けに記録することで表面形状が変化しないのは勿論のこ
と、その記録部分は出てきた赤外線吸収インキの色が白
色または淡色な為、目視が困難となり、かつ、非記録部
分は赤外線吸収能が弱く、記録部分が赤外線吸収能が増
加することにより赤外線リーダー及び/または赤外スコ
ープ赤外線により読み取りが可能である。
According to the invention described in claims 1 to 6, since information can be written by irradiating infrared rays, variable information can be recorded and the recorded information can be hidden without feeling unnaturalness. And, of course, the surface shape does not change by recording only on the intermediate layer of the medium by the laser beam, and the recorded portion has a white or light color of the infrared absorbing ink, which makes it difficult to see, In addition, the non-recorded portion has a weak infrared absorbing ability, and the recorded portion has an increased infrared absorbing ability, so that it can be read by an infrared reader and / or an infrared scope infrared ray.

【0040】さらに、請求項7〜9に係わる発明によれ
ば、不可視情報記録媒体の保護層はレーザービームを透
過できる限り、及び/または赤外スコープにより記録の
読み取りが可能な限り、その膜厚を厚くすることが可能
である。
Further, according to the inventions of claims 7 to 9, the protective layer of the invisible information recording medium has a film thickness as long as the laser beam can be transmitted and / or the recording can be read by an infrared scope. Can be thickened.

【0041】[0041]

【実施例】以下、本発明の一実施例を具体的に説明す
る。
EXAMPLE An example of the present invention will be specifically described below.

【0042】<実施例1>この実施例に係わる機械読み
取り可能な不可視情報記録媒体は、図1に示すように基
材1と、その表面に形成された以下に述べる赤外線吸収
インキ層2と、この赤外線吸収インキ層上に設けられた
感熱記録層3と保護層4とで、その主要部が構成されて
いるものである。以下、順に説明する。
<Embodiment 1> A machine-readable invisible information recording medium according to this embodiment includes a base material 1 and an infrared absorbing ink layer 2 formed on the surface of the base material 1 as shown below, as shown in FIG. The thermosensitive recording layer 3 and the protective layer 4 provided on the infrared absorbing ink layer constitute the main part. Hereinafter, they will be described in order.

【0043】 [赤外線吸収インキ] 染料(シアニン系染料) 0.5重量部 樹脂(ポリエステル系樹脂) 12.5重量部 溶剤(トルエン) 87重量部[Infrared absorbing ink] Dye (cyanine dye) 0.5 part by weight Resin (polyester resin) 12.5 parts by weight Solvent (toluene) 87 parts by weight

【0044】そして、この赤外線吸収インキを適用して
前期基材1上に膜厚10μmの赤外線吸収インキ層2を
設けた。
Then, by applying this infrared absorbing ink, an infrared absorbing ink layer 2 having a film thickness of 10 μm was provided on the base material 1 in the previous period.

【0045】その上に、アクリル系空中マイクロカプセ
ル樹脂エマルジョン(平均粒径0.5μm,固形分比3
3.6%)を10μmの厚みに塗布した。
On top of that, an acrylic airborne microcapsule resin emulsion (average particle size 0.5 μm, solid content ratio 3
3.6%) was applied to a thickness of 10 μm.

【0046】更に、赤外線を透過する性質を備えた保護
層4(日本触媒製 水系オーバーコート剤)を前記赤外
線吸収インキ層上に膜厚1〜2μmを設けた。
Further, a protective layer 4 (water-based overcoating agent manufactured by Nippon Shokubai Co., Ltd.) having a property of transmitting infrared rays was formed on the infrared ray absorbing ink layer in a thickness of 1 to 2 μm.

【0047】以上、実施例1で示した、不可視情報記録
媒体を表面側からレーザービームを照射したところ、得
られた記録部分は非記録部分とは区別がつかず目視がほ
とんど不可能であった。また、記録部分の赤外スコープ
での確認はできた。
As described above, when the invisible information recording medium shown in Example 1 was irradiated with the laser beam from the surface side, the obtained recorded portion was indistinguishable from the non-recorded portion and was hardly visible. . Also, the recorded part could be confirmed with an infrared scope.

【0048】<実施例2>この実施例に係わる不可視情
報記録媒体は、前記赤外吸収インキを以下に述べる第二
銅含有リン酸塩系白色結晶化合物を顔料とした赤外線吸
収インキに変えたことと、その為に実施例1に係わる赤
外線吸収インキ層よりも白色度を低下(極薄い青緑色を
呈した)させた点と、前記感熱記録層と、前記保護層と
の間に赤外線を透過する性質を備えたプロセスインキ
(東洋インキ製造社製 商品名FDOL)または前記赤
外線吸収インキと同色に色合わせをしたインキによる図
2の隠蔽層5を設けた点を除き実施例1に係わる不可視
情報記録媒体と略同一である。
<Example 2> In the invisible information recording medium according to this example, the infrared absorbing ink was changed to an infrared absorbing ink having a cupric phosphate-containing white crystalline compound described below as a pigment. For that reason, the whiteness is lower than that of the infrared absorbing ink layer according to Example 1 (exhibiting an extremely thin blue-green color), and infrared rays are transmitted between the heat-sensitive recording layer and the protective layer. Invisible information according to Example 1 except that the process ink (trade name: FDOL manufactured by Toyo Ink Mfg. Co., Ltd.) having the property to perform or the ink having the same color as the infrared absorbing ink is provided with the masking layer 5 of FIG. It is almost the same as the recording medium.

【0049】前記隠蔽層はベタまたは絵柄、地紋等でも
良く、絵柄、地紋等の場合はそのデザインは細かく、線
や点の隙間が狭いものが好ましい。
The concealing layer may be solid or a pattern, a tint block or the like. In the case of a pattern, tint block or the like, it is preferable that the design is fine and the gap between lines and dots is narrow.

【0050】以下、前記赤外線吸収インキについて説明
すると、まず、下記の組成を有する第二銅含有リン酸塩
系組成物について融解しかつこれを結晶化させて第二銅
含有リン酸塩系白色結晶化合物を求めた。
The infrared absorbing ink will be described below. First, a cupric-containing phosphate-based composition having the following composition is melted and crystallized to form a cupric-containing phosphate-based white crystal. The compound was sought.

【0051】[第二銅含有リン酸塩系組成物] P2 5 50.0重量% CuO 49.5重量% ZnO 0.5重量%[Copper-containing phosphate composition] P 2 O 5 50.0% by weight CuO 49.5% by weight ZnO 0.5% by weight

【0052】尚、この化合物について銅の管球(CuK
α)を用いてX線回折を行ったところ、回折角(2θ)
=28.14、30.07、34、44.01に強いピ
ークが現れ、結晶化されていることが確認された。
Regarding this compound, a copper tube (CuK
When X-ray diffraction was performed using α), the diffraction angle (2θ)
= 28.14, 30.07, 34, 44.01, strong peaks appeared, and it was confirmed that the crystals were crystallized.

【0053】次に、この第二銅含有リン酸塩系白色結晶
を粉砕して粉末化し、これを赤外線吸収性顔料として下
記組成の赤外線吸収インキを調製した。
Next, the cupric-containing phosphate-based white crystal was crushed into a powder, and this was used as an infrared absorbing pigment to prepare an infrared absorbing ink having the following composition.

【0054】 [赤外線吸収インキ] 顔料(第二銅含有リン酸塩系白色結晶化合物) 30重量部 塩酢酸ビニル系樹脂(積水化学工業社製 商品名エレックスA)10重量部 飽和ポリエステル(東洋紡績社製 商品名バイロン103) 5重量部 ポリウレタンエトラマー 12重量部 (日本ポリウレタン工業社製 商品名N−2304) イソシアート硬化剤 3重量部 トリエチレンジアミン 0.5重量部 溶剤(トルエン/メチルイソブチルケトン) 60重量部[Infrared absorbing ink] Pigment (cupric acid-containing phosphate white crystal compound) 30 parts by weight Vinyl acetate vinyl resin (trade name Elex A manufactured by Sekisui Chemical Co., Ltd.) 10 parts by weight Saturated polyester (Toyobo Co., Ltd.) Product name Byron 103) 5 parts by weight Polyurethane etramer 12 parts by weight (Nippon Polyurethane Industry Co., Ltd. product name N-2304) Isosiat curing agent 3 parts by weight Triethylenediamine 0.5 parts by weight Solvent (toluene / methyl isobutyl ketone) 60 parts by weight Department

【0055】そして、この赤外線吸収インキを適用して
前期基材1上に膜厚10μmの赤外線吸収インキ層2を
設けた。
Then, this infrared absorbing ink was applied to form an infrared absorbing ink layer 2 having a film thickness of 10 μm on the base material 1 in the previous period.

【0056】前記の不可視情報記録媒体においても、そ
の表面側からレーザービームを照射したところ、得られ
た記録部分は非記録部分とは実施例1以上に区別がつか
ず目視が不可能であった。また、記録部分の赤外スコー
プでの確認はできた。
Also in the above invisible information recording medium, when the laser beam was irradiated from the surface side, the obtained recorded portion was indistinguishable from the non-recorded portion as in Example 1 and could not be visually observed. . Also, the recorded part could be confirmed with an infrared scope.

【0057】<実施例3>この実施例に係わる不可視情
報記録媒体は、前記赤外吸収インキを以下に述べるナフ
タロシアニン系の染料を使用した赤外線吸収インキに変
えたことと、その為に実施例1に係わる赤外線吸収イン
キ層よりも白色度を低下(薄い茶褐色を呈した)させた
点と、前記感熱記録層に赤外線を透過する性質を備えた
茶褐色の染料または有色透明顔料を添加した感熱記録層
を設けた点を除き実施例1に係わる不可視情報記録媒体
と略同一である。
<Embodiment 3> The invisible information recording medium according to this embodiment is different from the infrared absorbing ink in that the infrared absorbing ink using a naphthalocyanine dye described below is used. Thermal recording in which a brown dye or a colored transparent pigment having the property of transmitting infrared rays to the heat-sensitive recording layer is added, and the whiteness is lower than that of the infrared-absorbing ink layer according to (1). It is substantially the same as the invisible information recording medium according to Example 1 except that a layer is provided.

【0058】 [赤外線吸収インキ] 顔料(ナフタロシアニン系染料) 5重量部 樹脂(ポリエステル系樹脂) 25重量部 溶剤(トルエン) 65重量部 (酢酸エチル) 5重量部[Infrared absorbing ink] Pigment (naphthalocyanine dye) 5 parts by weight Resin (polyester resin) 25 parts by weight Solvent (toluene) 65 parts by weight (ethyl acetate) 5 parts by weight

【0059】前記の不可視情報記録媒体において、その
表面は可視において茶褐色を呈しているが、その表面側
からレーザービームを照射したところ、得られた記録部
分は非記録部分とは区別がつかず目視がほとんど不可能
であった。また、記録部分の赤外スコープでの確認はで
きた。
In the above-mentioned invisible information recording medium, the surface thereof has a dark brown color in the visible, but when a laser beam is irradiated from the surface side, the obtained recorded portion is indistinguishable from the non-recorded portion and is visually observed. Was almost impossible. Also, the recorded part could be confirmed with an infrared scope.

【0060】[0060]

【発明の効果】請求項1〜6に係わる発明によれば、赤
外線を照射することで情報の書き込みができるので、可
変情報を記録でき、不自然さを感じさせずに記録情報を
隠蔽することができ、かつレーザービームにより媒体の
中間層だけに記録することで表面形状が変化しないのは
勿論のこと、その記録部分は出てきた赤外線吸収インキ
の色が白色または淡色な為、目視が困難となり、かつ、
非記録部分は赤外線吸収能が弱く、記録部分が赤外線吸
収能が増加することにより赤外線リーダー及び/または
赤外スコープ赤外線により読み取りが可能である。
According to the inventions according to claims 1 to 6, since information can be written by irradiating infrared rays, variable information can be recorded and the recorded information can be hidden without feeling unnatural. In addition, the surface shape does not change by recording only on the intermediate layer of the medium by the laser beam, and it is difficult to see it because the color of the infrared absorbing ink that appears is white or light at the recording part. And, and
The non-recorded portion has a weak infrared absorbing ability, and the recorded portion has an increased infrared absorbing ability, so that it can be read by an infrared reader and / or infrared scope infrared.

【0061】よって、記録された記録は察知することが
困難な為、記録の偽造、変造防止をより確実に行うこと
ができる。
Therefore, since it is difficult to detect the recorded record, it is possible to more reliably prevent forgery and alteration of the record.

【0062】請求項7〜9に係わる発明によれば、不可
視情報記録媒体の保護層はレーザービームを透過できる
限り、及び/または赤外スコープにより記録の読み取り
が可能な限り、その膜厚を厚くすることが可能である。
According to the inventions of claims 7 to 9, the protective layer of the invisible information recording medium is made thick as long as the laser beam can be transmitted and / or the recording can be read by an infrared scope. It is possible to

【0063】よって、膜強度を強くする事のみならず、
サーマルヘッドでは記録不可能となり、レーザービーム
による記録しかできなくなる為、サーマルヘッド等の熱
による記録の偽造、変造防止をより確実に行う事ができ
る。
Therefore, not only is the film strength increased,
Since recording cannot be performed with the thermal head and only recording with a laser beam is possible, it is possible to more reliably prevent forgery and alteration of recording due to heat from the thermal head or the like.

【0064】[0064]

【図面の簡単な説明】[Brief description of drawings]

【図1】実施例1に係わる不可視情報記録媒体の断面図
である。
FIG. 1 is a sectional view of an invisible information recording medium according to a first embodiment.

【図2】実施例2に係わる不可視情報記録媒体の断面図
である。
FIG. 2 is a sectional view of an invisible information recording medium according to a second embodiment.

【符号の説明】[Explanation of symbols]

1 基材 2 赤外線吸収インキ層 3 感熱記録層 4 保護層 5 隠蔽層 1 Base Material 2 Infrared Absorption Ink Layer 3 Thermal Recording Layer 4 Protective Layer 5 Concealment Layer

フロントページの続き (51)Int.Cl.5 識別記号 庁内整理番号 FI 技術表示箇所 B41M 5/26 5/28 B42D 15/00 341 C 8604−2C C09D 11/02 7415−4J 6956−2H B41M 5/18 112 Continuation of front page (51) Int.Cl. 5 Identification number Office reference number FI Technical display location B41M 5/26 5/28 B42D 15/00 341 C 8604-2C C09D 11/02 7415-4J 6956-2H B41M 5 / 18 112

Claims (9)

【特許請求の範囲】[Claims] 【請求項1】基材の表面に、赤外線吸収インキ層と、前
記赤外線吸収インキ層と同系色で、常温では赤外線を散
乱し、所定の温度以上の加熱で赤外線透過率が増大する
感熱記録層を積層し、更に前記感熱記録層を赤外透過材
料から構成される保護層で覆ったことを特徴とする不可
視情報記録媒体。
1. An infrared absorbing ink layer on the surface of a base material, and a thermosensitive recording layer having a similar color to the infrared absorbing ink layer, which scatters infrared rays at room temperature and increases infrared transmittance by heating above a predetermined temperature. And a heat-sensitive recording layer covered with a protective layer made of an infrared transmitting material.
【請求項2】基材の表面に、赤外線吸収インキ層と、常
温では赤外線を散乱し、所定の温度以上の加熱で赤外線
透過率が増大する感熱記録層を積層し、前記赤外線吸収
インキ層と同系色で赤外線透過性のインキからなる隠蔽
層で覆ったことを特徴とする不可視情報記録媒体。
2. An infrared absorbing ink layer and a heat sensitive recording layer which scatters infrared rays at room temperature and whose infrared transmittance increases by heating above a predetermined temperature are laminated on the surface of a base material, and the infrared absorbing ink layer and the infrared absorbing ink layer. An invisible information recording medium, characterized in that it is covered with a concealing layer made of an infrared-transparent ink of a similar color.
【請求項3】更に前記隠蔽層を赤外透過材料から構成さ
れる保護層で覆ったことを特徴とする請求項2記載の不
可視情報記録媒体。
3. The invisible information recording medium according to claim 2, wherein the concealing layer is further covered with a protective layer made of an infrared transmitting material.
【請求項4】感熱記録層が本質的に中空マイクロカプセ
ルから構成されることを特徴とする請求項1、2、3記
載の不可視情報記録媒体。
4. The invisible information recording medium according to claim 1, wherein the heat-sensitive recording layer is essentially composed of hollow microcapsules.
【請求項5】赤外線吸収インキ層が白色あるいは淡色で
あることを特徴とする請求項1、2、3記載の不可視情
報記録媒体。
5. The invisible information recording medium according to claim 1, wherein the infrared absorbing ink layer is white or light colored.
【請求項6】赤外線インキ層中の赤外吸収材料が五二酸
化リンを主成分とし、Fe2+及び/またはCu2+を含有
するリン酸白色結晶粉末から構成されることを特徴とす
る請求項1、2、3、5記載の不可視情報記録媒体。
6. The infrared absorbing material in the infrared ink layer is characterized by being composed of phosphoric acid white crystal powder containing phosphorus pentoxide as a main component and Fe 2+ and / or Cu 2+. The invisible information recording medium according to items 1, 2, 3, and 5.
【請求項7】請求項1記載の不可視情報記録媒体を取り
扱う情報記録方法であって、前記保護層側から赤外線を
照射し、感熱記録層を加熱することにより情報を記録す
ることを特徴とする不可視情報記録媒体の情報記録方
法。
7. An information recording method for handling an invisible information recording medium according to claim 1, wherein the information is recorded by irradiating infrared rays from the protective layer side and heating the heat-sensitive recording layer. Information recording method for invisible information recording medium.
【請求項8】請求項2、3記載の不可視情報記録媒体を
取り扱う情報記録方法であって、前記隠蔽層側から赤外
線を照射し、感熱記録層を加熱することにより情報を記
録することを特徴とする不可視情報記録媒体の情報記録
方法。
8. An information recording method for handling an invisible information recording medium according to claim 2 or 3, wherein information is recorded by irradiating infrared rays from the concealing layer side and heating the heat-sensitive recording layer. And an information recording method for an invisible information recording medium.
【請求項9】前記赤外線の照射による記録が赤外線リー
ダー及び/または赤外スコープにより読み取り可能なパ
ターンであることを特徴とする請求項7、8記載の不可
視情報記録媒体の情報記録方法。
9. The information recording method for an invisible information recording medium according to claim 7, wherein the recording by the irradiation of infrared rays is a pattern readable by an infrared reader and / or an infrared scope.
JP07672393A 1993-04-02 1993-04-02 Invisible information recording medium and information recording method for handling the same Expired - Fee Related JP3326859B2 (en)