JPH05179277A - Sliding member and sliding bush - Google Patents

Sliding member and sliding bush

Info

Publication number
JPH05179277A
JPH05179277A JP36016191A JP36016191A JPH05179277A JP H05179277 A JPH05179277 A JP H05179277A JP 36016191 A JP36016191 A JP 36016191A JP 36016191 A JP36016191 A JP 36016191A JP H05179277 A JPH05179277 A JP H05179277A
Authority
JP
Japan
Prior art keywords
sliding
coating
cylinder
bush
fiber
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP36016191A
Other languages
Japanese (ja)
Other versions
JP3110537B2 (en
Inventor
Yasunobu Shimano
康信 島野
Motoyuki Tanaka
元行 田中
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kurashiki Kako Co Ltd
Original Assignee
Kurashiki Kako Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kurashiki Kako Co Ltd filed Critical Kurashiki Kako Co Ltd
Priority to JP36016191A priority Critical patent/JP3110537B2/en
Publication of JPH05179277A publication Critical patent/JPH05179277A/en
Application granted granted Critical
Publication of JP3110537B2 publication Critical patent/JP3110537B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

PURPOSE:To provide a sliding member having a specific constitution, low torsional rigidity and low rotational torque, usable over a long period without lubrication, having excellent corrosion resistance to saline solution, etc., and useful for the connecting part of a suspension rod of automobile, etc. CONSTITUTION:The objective sliding member is composed of a member A having at least the sliding face 2a made of a polyamide resin containing 10-50wt.% of reinforcing fiber and a member B having a sliding face 2b made of an electro-deposition coating layer formed on a metallic member. The reinforcing fiber of the member A is usually glass fiber, carbon fiber, etc., and the fiber is preferably compounded with fluororesin powder, etc., to improve the lubricity. The electro-deposition coating of the sliding face of the member B is carried out by using e.g. a cationic epoxy resin coating and an anionic polybutadiene resin coating. The surface of the metal is preferably coated with a coating film of iron phosphate, etc., before electro-deposition coating to improve the rust-proofing property and the durability of the coating film.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は、主として自動車等輸送
用機器の摺動部材を構成する摺動体及び摺動ブッシュに
関するものである。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention mainly relates to a sliding body and a sliding bush which constitute a sliding member of transportation equipment such as automobiles.

【0002】[0002]

【従来の技術】自動車のトルクロッド、サスペンション
ロッドなどの連結部など、自動車の構成部品間を連結さ
せる摺動部材には無給油で、摺動抵抗が小さく、耐久
性、耐食性に優れるものがメインテナンスフリーの点で
求められている。これらの要求から、上記諸特性を満足
させる摺動部材の組合せ、及びそれを使用した摺動ブッ
シュが求められている。
2. Description of the Related Art A sliding member for connecting components of an automobile, such as a connecting portion of a torque rod and a suspension rod of an automobile, is oil-free, has a small sliding resistance, and has excellent durability and corrosion resistance. Free is required. From these requirements, a combination of sliding members satisfying the above various characteristics and a sliding bush using the same are required.

【0003】従来、例えば摺動ブッシュにおいては、金
属製の円柱状連結ピンの外周にポリアミド、ポリアセタ
ールなどの摺動筒を形成し、この摺動筒と外筒との間に
弾性体を介装したものが知られている(実公昭55-45149
号)。
Conventionally, for example, in a sliding bush, a sliding cylinder made of polyamide, polyacetal or the like is formed on the outer periphery of a metal cylindrical connecting pin, and an elastic body is interposed between the sliding cylinder and the outer cylinder. It is known that
issue).

【0004】[0004]

【発明が解決しようとする課題】本発明は、従来よりも
更に捩り剛性を下げるとか低回転トルクとすると共に、
無給油で長期の使用が可能であり、しかも、塩水等に対
する耐食性に優れた摺動体及び摺動ブッシュ、例えば自
動車サスペンションブッシュを提供しようとするもので
ある。
SUMMARY OF THE INVENTION According to the present invention, the torsional rigidity is further reduced and the rotational torque is reduced as compared with the conventional one.
An object of the present invention is to provide a sliding body and a sliding bush, such as an automobile suspension bush, which can be used for a long period of time without lubrication and have excellent corrosion resistance against salt water and the like.

【0005】[0005]

【課題を解決するための手段】上記課題を検討した結
果、下記構造の摺動体及び摺動ブッシュとした。すなわ
ち、互いに摺動する二つの部材で、一方の部材の少なく
とも摺動面が補強短繊維を10〜50重量%含むポリアミド
樹脂であり、他方の部材の摺動面が金属部材の電着塗装
面である部材の組合せからなる摺動体とした。
As a result of examining the above problems, a sliding body and a sliding bush having the following structures were obtained. That is, two members that slide with each other, at least the sliding surface of one member is a polyamide resin containing 10 to 50% by weight of reinforcing short fibers, and the sliding surface of the other member is an electrodeposition coated surface of a metal member. The sliding body is composed of a combination of the members.

【0006】ここで、ポリアミド樹脂としては、ナイロ
ン(6、11、12、6,6)等が使用できる。補強短繊維とし
ては、ガラス繊維、炭素繊維、アラミド繊維などが使用
できる。更に、これらの繊維強化物には潤滑性向上のた
め、フッソ樹脂パウダーや二硫化モリブデンを配合した
ものが好適に使用できる。また、電着塗装前の金属の表
面は素地のままでもよいが、塗装前の防錆及び塗膜の耐
久性のために、リン酸鉄、リン酸亜鉛、リン酸亜鉛カル
シウムなどの皮膜を形成するとよい。電着塗装としては
カチオン型エポキシ樹脂系塗料の他にも、アニオン型の
ポリブタジエン樹脂やポリエステル樹脂等の塗料が使用
できる。
Here, nylon (6, 11, 12, 6, 6) or the like can be used as the polyamide resin. As the reinforcing short fibers, glass fibers, carbon fibers, aramid fibers and the like can be used. Further, in order to improve the lubricity, it is possible to suitably use those fiber reinforced materials containing fluorine resin powder or molybdenum disulfide. The surface of the metal before electrodeposition coating may be left as it is, but a film of iron phosphate, zinc phosphate, zinc calcium phosphate, etc. is formed for rust prevention and durability of the coating before coating. Good to do. As the electrodeposition coating, in addition to cationic epoxy resin-based coatings, coatings such as anionic polybutadiene resins and polyester resins can be used.

【0007】また、一方の部材の少なくとも摺動面が補
強短繊維を10〜50重量%含むポリアミド樹脂であり、他
方の部材の摺動面が金属部材のフッソ樹脂被覆面である
部材の組合せからなる摺動体とした。
In addition, at least the sliding surface of one member is made of a polyamide resin containing 10 to 50% by weight of reinforcing short fibers, and the sliding surface of the other member is made of a metal resin such as a fluorine resin coated surface. It was a sliding body.

【0008】ここで、フッ素樹脂としてはPTFE(ポリテ
トラフルオロエチレン)、ETFE(エチレン/テトラフルオ
ロエチレン共重合体)、PFA(テトラフルオロエチレン/
アルキルビニルエーテルランダム共重合体)、PCTFE(ポ
リクロロトリフルオロエチレン)、TFEHP(テトラフルオ
ロエチレン/ヘキサフルオロプロピレン共重合体)など
が使用できる。このフッ素樹脂にも潤滑性向上のため、
二硫化モリブデンやグラファイトなどを適宜混合するこ
とができる。
Here, as the fluororesin, PTFE (polytetrafluoroethylene), ETFE (ethylene / tetrafluoroethylene copolymer), PFA (tetrafluoroethylene /
Alkyl vinyl ether random copolymer), PCTFE (polychlorotrifluoroethylene), TFEHP (tetrafluoroethylene / hexafluoropropylene copolymer) and the like can be used. To improve the lubricity of this fluororesin,
Molybdenum disulfide, graphite and the like can be appropriately mixed.

【0009】これら摺動体は、より具体的な態様として
は、摺動面が曲面である内軸体とその外周の摺動筒から
なるものである。摺動ブッシュは上記摺動体の摺動筒の
外方に弾性筒と硬質外筒とを順次設けた構造である。
In a more specific form, these sliding bodies are composed of an inner shaft having a curved sliding surface and a sliding cylinder on the outer periphery thereof. The sliding bush has a structure in which an elastic cylinder and a hard outer cylinder are sequentially provided outside the sliding cylinder of the sliding body.

【0010】[0010]

【作用】このような構造の摺動体及び摺動ブッシュは、
一方の部材の繊維強化されたポリアミド樹脂摺動面が高
強度及び低い摺動抵抗を持ち、また、他方の部材の摺動
面の金属部材の電着塗装面あるいはフッソ樹脂被覆面が
塩水等に対する耐食性と低い摺動抵抗をもつので、円筒
体のような摺動曲面の場合、低回転トルクで摺動可能か
つ耐食性に優れたものとなる。
[Function] The sliding body and sliding bush having such a structure are
The fiber reinforced polyamide resin sliding surface of one member has high strength and low sliding resistance, and the sliding surface of the other member has a metal member electrodeposition coated surface or a fluorine resin coated surface against salt water, etc. Since it has corrosion resistance and low sliding resistance, in the case of a sliding curved surface such as a cylindrical body, it can be slid with a low rotational torque and is excellent in corrosion resistance.

【0011】更に、この摺動体の組合せがイオン化傾向
に基づく電蝕により起こるとされる塗膜のふくれ(blist
er)などを発生させないので、その結果として長期間に
亘って初期と変わらぬ製品性能を保持することができ
る。
Further, the blist of the coating film, which is said to be caused by the electrolytic corrosion based on the ionization tendency, is caused by the combination of the sliding members.
As a result, it is possible to maintain the product performance unchanged from the initial state for a long period of time.

【0012】[0012]

【実施例】【Example】

実施例1,2(金属部材電着塗装) 図1は一方の部材Aが合成樹脂で、他方の部材Bが金属
であり、これら部材A,B間は互いに摺動する構造の摺
動体の例である。一方の部材Aは摺動面2aを含む全体が
炭素繊維の短繊維を30重量%含む6,6ナイロン樹脂製で
ある。6,6ナイロン樹脂には市販品の2銘柄(東レ(株)製
トレカ,実施例1、東レ(株)製アミラン,実施例2)を使
用した。また、他方の部材Bは鋼製であって、その表面
の摺動面2bはエポキシ系カチオン電着塗装を施してい
る。
Examples 1 and 2 (Electrodeposition of metal members) FIG. 1 shows an example of a sliding body having a structure in which one member A is a synthetic resin and the other member B is a metal, and the members A and B slide against each other. Is. On the other hand, the entire member A including the sliding surface 2a is made of 6,6 nylon resin containing 30% by weight of short carbon fibers. As the 6,6 nylon resin, two commercially available products (Toray Industries, Inc., trading card, Example 1, Toray Industries, Inc., Amiran, Example 2) were used. The other member B is made of steel, and the sliding surface 2b on its surface is coated with an epoxy-based cationic electrodeposition coating.

【0013】カチオン電着塗装の工程は次のように行な
った。まず初めに金属製部材Bを有機溶剤で脱脂、酸除
錆した後、その表面にリン酸亜鉛カルシウム皮膜を形成
し、その表面にカチオン電着プライマー塗料(商品名パ
ワーコート)を用いて電着塗膜を形成した後、190℃で30
分間焼付乾燥を行なった。
The process of cationic electrodeposition coating was performed as follows. First, the metal member B is degreased with an organic solvent and acid rust removed, and then a zinc calcium phosphate film is formed on the surface of the metal member B, and a cation electrodeposition primer coating (trade name: Power Coat) is used on the surface to electrodeposition After forming the coating film, at 190 ℃ 30
It was baked and dried for 1 minute.

【0014】この実施例における回転トルクは表1中に
も示したが、テフロンクロスを部材A,B間に用いた場
合の54kg・cmに近いものとなった。テフロンクロスを使
用した場合よりも製造工程が少なくてすみ、コストも安
価で、無給油での摺動を可能としたのである。これは、
例えば後に詳細に説明するが、内筒と外筒間に摺動樹脂
及び弾性体が存在する弾性ブッシュやピロボールブッシ
ュ、更にはボールジョイント等に実施が可能である。
The rotation torque in this embodiment is shown in Table 1 and is close to 54 kg.cm when Teflon cloth is used between the members A and B. The number of manufacturing processes is smaller than when Teflon cloth is used, the cost is low, and sliding without lubrication is possible. this is,
For example, as will be described in detail later, the present invention can be applied to an elastic bush or a pillow ball bush in which a sliding resin and an elastic body are present between an inner cylinder and an outer cylinder, and a ball joint.

【0015】実施例3,4(金属部材フッソ樹脂被覆) 前記実施例で部材Bの摺動面2bの表面塗装であるカチオ
ン電着塗装に代えて、フッソ樹脂被覆を行った。フッソ
樹脂は表1中に示す市販のデフリックコート(川邑研究
所製)を用いた。フッソ樹脂被覆の工程は次のように行
った。まず初めに、金属製部材Bを有機溶剤で脱脂、酸
除錆後、その表面へ常法によりリン酸塩皮膜を形成し
た。その後適度に希釈したデフリックコートをそれぞれ
スプレーコーティングし、150℃で30分間焼付けをし
た。
Examples 3 and 4 (metal member fluorine resin coating) Instead of the cationic electrodeposition coating which is the surface coating of the sliding surface 2b of the member B in the above examples, fluorine resin coating was performed. As the fluorine resin, a commercially available deflick coat (manufactured by Kawamura Laboratory) shown in Table 1 was used. The step of coating with the fluorine resin was performed as follows. First, the metal member B was degreased with an organic solvent and acid-rusted, and then a phosphate film was formed on the surface thereof by a conventional method. After that, each of the appropriately diluted deflick coats was spray-coated and baked at 150 ° C. for 30 minutes.

【0016】この金属製部材Bと、前記実施例における
摺動面2aが炭素繊維の短繊維を30重量%含む2銘柄の6,
6ナイロン樹脂製の部材Aとからなる摺動体の回転トル
クの測定結果も表1中に示した。この例でも回転トルク
がテフロンクロスを部材A,B間に用いた場合に近いも
のとなっている。表1中にはこの外、比較例としてノー
マル、すなわち表面処理が施されていない素地のままの
もの(比較例1)と、従来の硬質クロムメッキを施したも
の(比較例2)を示した。
This metal member B and two brands of 6, whose sliding surface 2a in the above embodiment contains 30% by weight of short carbon fibers,
Table 1 also shows the measurement results of the rotational torque of the sliding body composed of the member A made of 6 nylon resin. Also in this example, the rotational torque is close to that when the Teflon cloth is used between the members A and B. In addition to this, Table 1 also shows, as comparative examples, a normal product, that is, an untreated substrate (Comparative Example 1) and a conventional hard chrome plated product (Comparative Example 2). ..

【0017】[0017]

【表1】 [Table 1]

【0018】防錆試験 上記実施例1の金属製部材Bが電着塗装されたもの、及
び、実施例3のフッソ樹脂被覆が施されたものをJIS Z
2371により塩水噴霧試験を行った。同時に比較例として
素地のままのもの(比較例1)と、硬質クロムメッキが施
されたもの(比較例3)についても行った。その結果を表
2に示す。
Anticorrosion test JIS Z of the metal member B of the above-mentioned Example 1 electrodeposited and that of Example 3 coated with the fluorine resin are JIS Z
A salt spray test was performed according to 2371. At the same time, as a comparative example, the test was carried out for the raw material (Comparative Example 1) and the hard chrome plated product (Comparative Example 3). The results are shown in Table 2.

【0019】素地だけのものや硬質クロムメッキでは48
時間以内で赤錆が発生しているのに対して、本発明の電
着塗装及びフッソ樹脂被覆が施されたものは480時間経
過しても赤錆の発生がなかった。
48 for bare metal or hard chrome plating
While red rust was generated within the time, the electrodeposition coating and the fluorine resin coating of the present invention did not generate red rust even after 480 hours.

【0020】[0020]

【表2】 [Table 2]

【0021】図2〜5に本発明の実施態様を例示した。
図2は弾性ブッシュに実施した例であって、この例では
内軸体3が前記摺動体の金属製部材Bに相当し、中ほど
に太径部分を有している。その表面の摺動面2bは、これ
までに説明した表面塗装である電着塗装又はフッソ樹脂
被覆を施している。その外周の摺動筒1は前記部材Aに
相当し炭素繊維の短繊維を含む6,6ナイロン樹脂製であ
る。これは補強短繊維を10〜50重量%含む他のポリアミ
ド樹脂でも構わない。これらの部材で構成された摺動筒
の外方にゴム弾性筒4とその外周に鋼製の硬質外筒5と
を順次設けている。
2 to 5 illustrate the embodiments of the present invention.
FIG. 2 shows an example in which the elastic bush is used. In this example, the inner shaft body 3 corresponds to the metal member B of the sliding body, and has a large diameter portion in the middle. The sliding surface 2b on the surface is subjected to electrodeposition coating or fluorine resin coating, which is the surface coating described so far. The sliding cylinder 1 on the outer periphery thereof is made of 6,6 nylon resin corresponding to the member A and containing short carbon fibers. This may be another polyamide resin containing 10 to 50% by weight of reinforcing short fibers. A rubber elastic cylinder 4 and a hard outer cylinder 5 made of steel are sequentially provided on the outer side of a sliding cylinder formed of these members.

【0022】図3も弾性ブッシュの例であるが、前記図
2の例とほぼ同じ構造で、ポリアミド樹脂製の摺動筒1
の内部に、補強のために金属製の中間筒6を一体で設け
ている。
FIG. 3 also shows an example of the elastic bush, but the sliding cylinder 1 made of polyamide resin has substantially the same structure as the example of FIG.
Inside, a metal intermediate cylinder 6 is integrally provided for reinforcement.

【0023】図4はピロボールブッシュの例である。内
軸体3の摺動面2bが曲面であり、この面に電着塗装又は
フッソ樹脂被覆を施している。その外周の摺動筒1は前
記部材Aに相当し炭素繊維の短繊維を含む6,6ナイロン
樹脂製である。中間筒6を設けた点、その外周に弾性筒
4と鋼製の硬質外筒5とを順次設けた点は図3に示した
ものと同様である。
FIG. 4 shows an example of a pillow ball bush. The sliding surface 2b of the inner shaft body 3 is a curved surface, and this surface is subjected to electrodeposition coating or fluorine resin coating. The sliding cylinder 1 on the outer periphery thereof is made of 6,6 nylon resin corresponding to the member A and containing short carbon fibers. The point that the intermediate cylinder 6 is provided and that the elastic cylinder 4 and the hard outer cylinder 5 made of steel are sequentially provided on the outer periphery thereof are the same as those shown in FIG.

【0024】図5はボールジョイントの例である。金属
ボールスタッド7の基部側球面がこれまでの例と同様の
摺動面2bであって、電着塗装又はフッソ樹脂被覆を施し
ている。摺動面2aで摺動する摺動筒1は球状の外金具8
との間に補強短繊維を含むポリアミド樹脂で形成されて
いる。
FIG. 5 shows an example of a ball joint. The spherical surface on the base side of the metal ball stud 7 is the sliding surface 2b similar to the above-mentioned examples, and is subjected to electrodeposition coating or fluorine resin coating. The sliding cylinder 1 sliding on the sliding surface 2a is a spherical outer metal fitting 8
It is formed of a polyamide resin containing reinforcing short fibers between and.

【0025】[0025]

【発明の効果】本発明によって、捩り剛性が低く、低回
転トルクであり、無給油で長期の使用が可能で、しか
も、塩水等に対する耐食性に優れた摺動体及び摺動ブッ
シュの提供が可能となった。そこで、これによりトルク
ロッド、サスペンションロッドなどを安価で低回転トル
クかつ長寿命なものとすることができた。
According to the present invention, it is possible to provide a sliding body and a sliding bush which have low torsional rigidity, low rotational torque, can be used for a long time without lubrication, and have excellent corrosion resistance against salt water and the like. became. Therefore, this makes it possible to reduce the cost of the torque rod, suspension rod, etc. at low rotation torque and long life.

【図面の簡単な説明】[Brief description of drawings]

【図1】摺動体の断面図である。FIG. 1 is a cross-sectional view of a sliding body.

【図2】弾性ブッシュの断面図である。FIG. 2 is a sectional view of an elastic bush.

【図3】弾性ブッシュの断面図である。FIG. 3 is a sectional view of an elastic bush.

【図4】ピロボールブッシュの断面図である。FIG. 4 is a sectional view of a pillow ball bush.

【図5】ボールジョイントの断面図である。FIG. 5 is a sectional view of a ball joint.

【符号の説明】[Explanation of symbols]

1 摺動筒 2a 摺動面 2b 摺動面 3 内軸体 4 弾性筒 5 硬質外筒 6 中間筒 7 金属ボールスタッド 8 外金具 1 Sliding cylinder 2a Sliding surface 2b Sliding surface 3 Inner shaft body 4 Elastic cylinder 5 Hard outer cylinder 6 Intermediate cylinder 7 Metal ball stud 8 Outer fitting

フロントページの続き (51)Int.Cl.5 識別記号 庁内整理番号 FI 技術表示箇所 C10M 125:02 125:28 149:18) C10N 20:06 B 8217−4H 30:06 30:12 40:02 40:04 50:08 Continuation of the front page (51) Int.Cl. 5 Identification number Office reference number FI technical display location C10M 125: 02 125: 28 149: 18) C10N 20:06 B 8217-4H 30:06 30:12 40:02 40:04 50:08

Claims (4)

【特許請求の範囲】[Claims] 【請求項1】 互いに摺動する二つの部材で、一方の部
材の少なくとも摺動面が補強短繊維を10〜50重量%含む
ポリアミド樹脂であり、他方の部材の摺動面が金属部材
の電着塗装面である部材の組合せからなる摺動体。
1. Two members that slide with each other, at least the sliding surface of one member being a polyamide resin containing 10 to 50% by weight of reinforcing short fibers, and the sliding surface of the other member being a metal member. A sliding body consisting of a combination of members that are coated surfaces.
【請求項2】 互いに摺動する二つの部材で、一方の部
材の少なくとも摺動面が補強短繊維を10〜50重量%含む
ポリアミド樹脂であり、他方の部材の摺動面が金属部材
のフッソ樹脂被覆面である部材の組合せからなる摺動
体。
2. Two members that slide with each other, at least the sliding surface of one member being a polyamide resin containing 10 to 50% by weight of reinforcing short fibers, and the sliding surface of the other member being a metal member. A sliding body made of a combination of members that are resin coated surfaces.
【請求項3】 摺動体の摺動面が曲面である内軸体とそ
の外周の摺動筒からなる請求項1又は2記載の摺動体。
3. The sliding body according to claim 1, which comprises an inner shaft having a curved sliding surface and a sliding cylinder on the outer periphery of the inner shaft.
【請求項4】 摺動筒の外方に弾性筒と硬質外筒とを順
次設けた請求項3記載の摺動体からなる摺動ブッシュ。
4. A sliding bush comprising the sliding body according to claim 3, wherein an elastic cylinder and a hard outer cylinder are sequentially provided outside the sliding cylinder.
JP36016191A 1991-12-27 1991-12-27 Sliding body Expired - Lifetime JP3110537B2 (en)