JP3394332B2 - Burring processing method - Google Patents

Burring processing method

Info

Publication number
JP3394332B2
JP3394332B2 JP20073894A JP20073894A JP3394332B2 JP 3394332 B2 JP3394332 B2 JP 3394332B2 JP 20073894 A JP20073894 A JP 20073894A JP 20073894 A JP20073894 A JP 20073894A JP 3394332 B2 JP3394332 B2 JP 3394332B2
Authority
JP
Japan
Prior art keywords
punch
burring
tubular body
die
hole
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP20073894A
Other languages
Japanese (ja)
Other versions
JPH0857563A (en
Inventor
正吾 楠元
浩 直井
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toyota Motor Corp
Original Assignee
Toyota Motor Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toyota Motor Corp filed Critical Toyota Motor Corp
Priority to JP20073894A priority Critical patent/JP3394332B2/en
Publication of JPH0857563A publication Critical patent/JPH0857563A/en
Application granted granted Critical
Publication of JP3394332B2 publication Critical patent/JP3394332B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は、管体の膨出部にバーリ
ング加工を行う方法に関し、とくに膨出部を形成する際
の管体の変形を防止することが可能なバーリング加工方
法に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a method for burring a bulging portion of a tubular body, and more particularly to a burring method capable of preventing deformation of the tubular body when forming the bulging portion.

【0002】[0002]

【従来の技術】管材にバーリング加工を行うには、予め
管材に外方に膨出する膨出部を形成することが必要であ
る。管材に、外方に膨出する膨出部を形成する技術の一
つとして、高圧の液圧を用いる液圧バルジ加工法が知ら
れている。また、液圧を用いることなく、管材の一部を
外方に膨出させる技術は、特開昭59−19025号公
報に開示されている。
2. Description of the Related Art In order to perform a burring process on a pipe material, it is necessary to previously form a bulging portion that bulges outward on the pipe material. As one of the techniques for forming a bulged portion that bulges outward in a pipe material, a hydraulic bulge processing method using high-pressure hydraulic pressure is known. Further, a technique of bulging a part of a pipe material outward without using hydraulic pressure is disclosed in Japanese Patent Laid-Open No. 59-19025.

【0003】[0003]

【発明が解決しようとする課題】しかし、上記の特開昭
59−19025号公報の加工方法の場合は、単に半球
状のプラグにより管体を内面から押圧して膨出部を形成
した後、バーリング加工を行うので、膨出部の成形時に
管体が変形し、管体の真円度等がくずれてしまうという
問題がある。
However, in the case of the processing method disclosed in Japanese Patent Laid-Open No. 59-19025, the hemispherical plug simply presses the tubular body from the inner surface to form the bulging portion, Since the burring process is performed, there is a problem that the tubular body is deformed when the bulging portion is formed, and the roundness and the like of the tubular body are lost.

【0004】本発明の目的は、膨出部の成形の際に、膨
出部に起因する管体の変形を防止することが可能なバー
リング加工方法を提供することにある。
An object of the present invention is to provide a burring method capable of preventing the deformation of the tubular body due to the bulging portion when forming the bulging portion.

【0005】[0005]

【課題を解決するための手段】この目的を達成するため
の本発明に係るバーリング加工方法は、つぎのように構
成されている。 (1) 管体を、内周面に形成された横穴と該横穴と同
一円周上で周方向に延び両端が前記横穴に接続された拡
管溝とを有するダイスと、パンチガイドとの間にセット
する工程と、 カムと圧縮パンチを同時に下降させ、該圧
縮パンチで前記管体を軸方向に押圧し、前記管体を前記
拡管溝に向けて膨出させて拡径部を形成しながら、前記
カムによりパンチを移動させて前記管体を前記横穴に向
けて膨出させ、膨出部を形成する工程と、を有するバー
リング加工方法。 (2) 前記拡管溝の断面積と前記横穴の断面積とは
ぼ等し(1)記載のバーリング加工方法。
A burring method according to the present invention for achieving this object is constructed as follows. (1) The tubular body has a horizontal hole formed on the inner peripheral surface and the same as the horizontal hole.
An expansion that extends in the circumferential direction on one circumference and has both ends connected to the lateral holes.
Set between the die having the tube groove and the punch guide
And the cam and compression punch are lowered at the same time.
The tube body is pressed in the axial direction with a compression punch, and the tube body is
While bulging toward the expansion groove to form the expanded diameter portion,
Move the punch with a cam to direct the tube to the lateral hole.
Burring and bulging to form a bulging portion . (2) the tube expansion groove cross-sectional area and have equal ho <br/> pot and the cross-sectional area of the lateral hole (1) burring method according.

【0006】[0006]

【作用】上記(1)のバーリング加工方法においては、
管体を、内周面に形成された横穴と内周面の横穴と同一
円周上で周方向に延び両端が横穴に接続された拡管溝と
を有するダイスに挿入し、圧縮パンチで管体を軸方向に
押圧し拡径部を形成しながらカムによりパンチを移動さ
せて膨出部を形成するようにしたので、膨出部の成形時
には膨出部に起因する管体の変形を防止することができ
る。上記(2)のバーリング加工方法においては管体
の真円度ずれおよび中心ずれを防止することができる
In the burring method of (1) above,
The tubular body is the same as the lateral hole formed on the inner peripheral surface and the inner peripheral surface.
A pipe expansion groove that extends in the circumferential direction on the circumference and has both ends connected to lateral holes.
Insert into a die with a
The punch is moved by the cam while pressing to form the expanded diameter part.
When forming the bulging part, the bulging part is formed by
Can prevent the deformation of the tube due to the bulge
It In the burring method (2), it is possible to prevent the roundness deviation and the center deviation of the tube.

【0007】[0007]

【実施例】図1ないし図7は、本発明の一実施例を示し
ている。まず、本発明を実施するための加工装置につい
て説明する。図1において、10は張り出し成形機を示
している。張り出し成形機10は、上部ダイス11aと
下部ダイス11bとからなるダイス11を有している。
上部ダイス11aと下部ダイス11bは、締結されてい
る。下部ダイス11bは、ベース13に固定されてい
る。ダイス11には、上下方向に延びる挿入穴14が形
成されている。挿入穴14の内周面には、外方に延びる
横穴15が形成されている。横穴15は、後述する膨出
部2を成形するものであり、径がDに設定され、深さが
1 に設定されている。横穴15は、上部ダイス11a
と下部ダイス11bの双方にまたがって形成されてい
る。
1 to 7 show an embodiment of the present invention. First, a processing apparatus for carrying out the present invention will be described. In FIG. 1, reference numeral 10 indicates an overhang molding machine. The overhang molding machine 10 has a die 11 including an upper die 11a and a lower die 11b.
The upper die 11a and the lower die 11b are fastened together. The lower die 11b is fixed to the base 13. The die 11 has an insertion hole 14 extending vertically. A lateral hole 15 extending outward is formed on the inner peripheral surface of the insertion hole 14. The lateral hole 15 is for molding a bulging portion 2 described later, and has a diameter set to D and a depth set to H 1 . The horizontal hole 15 is the upper die 11a.
And the lower die 11b.

【0008】挿入穴14の内周面には、周方向に延びる
拡管溝16が形成されている。拡管溝16は、横穴15
と同一円周上に位置している。拡管溝16は、幅がWに
設定され深さがH2 に設定されている。拡管溝16は、
本実施例では周方向全周に延びているが、横穴15と対
向する位置のみに設ける構成としてもよい。拡管溝16
の両端は、横穴15に滑らかに接続されている。図1に
示す様に断面で見た場合、ダイス11の横穴15と拡管
溝16の面積は等しくなっている。挿入穴14には、パ
ンチガイド17が配置されている。パンチガイド17の
上半分は、円筒部17aに形成されている。パンチガイ
ド17の外周面と挿入穴14の内周面との間には、管体
1を挿入するための隙間が形成されている。
A pipe expanding groove 16 extending in the circumferential direction is formed on the inner peripheral surface of the insertion hole 14. Expansion groove 16 has a horizontal hole 15
It is located on the same circumference as. The expansion groove 16 has a width set to W and a depth set to H 2 . The expansion groove 16 is
In this embodiment, it extends all around the circumferential direction, but it may be provided only at a position facing the lateral hole 15. Expansion groove 16
Both ends of are connected smoothly to the lateral holes 15. When viewed in a cross section as shown in FIG. 1, the lateral holes 15 of the die 11 and the expansion groove 16 have the same area. A punch guide 17 is arranged in the insertion hole 14. The upper half of the punch guide 17 is formed in the cylindrical portion 17a. A gap for inserting the tubular body 1 is formed between the outer peripheral surface of the punch guide 17 and the inner peripheral surface of the insertion hole 14.

【0009】パンチガイド17の円筒部17aの内側に
は、半径方向に移動可能なパンチ18が配置されてい
る。パンチガイド17の円筒部17aには、パンチ18
が出入り可能な穴17bが形成されている。パンチ18
は、ダイス11の横穴15に対向して配置されている。
パンチ18には、横穴15内に進入可能な凸部18aが
形成されている。パンチ18の凸部18aと反対側に
は、傾斜面18bが形成されている。パンチガイド17
の円筒部17aの内側には、パンチ18の傾斜面18b
と摺接可能な傾斜面19aを有するカム19が配置され
ている。円筒部17aの底面には、カム19の先端部を
逃がすための凹部17cが形成されている。
Inside the cylindrical portion 17a of the punch guide 17, a punch 18 which is movable in the radial direction is arranged. The punch 18 is attached to the cylindrical portion 17a of the punch guide 17.
A hole 17b is formed so that the can enter and exit. Punch 18
Are arranged so as to face the lateral holes 15 of the die 11.
The punch 18 is formed with a convex portion 18 a that can enter the lateral hole 15. An inclined surface 18b is formed on the side of the punch 18 opposite to the convex portion 18a. Punch guide 17
The inside of the cylindrical portion 17a of the punch 18 has an inclined surface 18b of the punch 18.
A cam 19 having an inclined surface 19a capable of sliding contact with is arranged. A concave portion 17c is formed on the bottom surface of the cylindrical portion 17a to allow the tip portion of the cam 19 to escape.

【0010】パンチガイド17の円筒部17aの底面側
には、パンチリターンスプリング20が固定されてい
る。パンチリターンスプリング20は、例えば板ばねか
ら構成されている。パンチリターンスプリング20の自
由端は、パンチ18の下面側と連結されている。円筒部
17aの底面側には、パンチリターンスプリング20が
変位するための逃げ穴17dが形成されている。パンチ
18は、カム19の押圧により傾斜面18bがカム19
の傾斜面19aと摺接し、ダイス11の横穴15に向っ
て移動するようになっている。パンチリターンスプリン
グ20は、横穴15側に移動したパンチ18を円筒部1
7a内に戻す機能を有する。
A punch return spring 20 is fixed to the bottom surface side of the cylindrical portion 17a of the punch guide 17. The punch return spring 20 is composed of, for example, a leaf spring. The free end of the punch return spring 20 is connected to the lower surface side of the punch 18. An escape hole 17d for displacing the punch return spring 20 is formed on the bottom surface side of the cylindrical portion 17a. In the punch 18, the inclined surface 18 b is pressed by the cam 19 so that the cam 19
It is slidably in contact with the inclined surface 19a of the die 11 and moves toward the lateral hole 15 of the die 11. The punch return spring 20 moves the punch 18 moved to the side of the lateral hole 15 into the cylindrical portion 1.
It has a function of returning to the inside of 7a.

【0011】パンチガイド17の外周には、圧縮パンチ
21が設けられている。圧縮パンチ21は、圧縮スプリ
ング22を介してダイス11の上方に位置する昇降ベー
ス23に支持されている。昇降ベース23には、油圧シ
リンダ等の駆動手段(図示略)か連結されている。圧縮
パンチ21の一方は、ダイス11の挿入穴14の内周面
とパンチガイド17の円筒部17aの外周面との間の隙
間に進入可能となっている。カム19の他方は、ベース
23に固定されている。昇降ベース23の移動により、
カム19によってパンチ18が押圧される際には、ダイ
ス11の挿入穴14に挿入された管体1が同時に圧縮パ
ンチ21によって軸方向に押圧されるようになってい
る。
A compression punch 21 is provided on the outer periphery of the punch guide 17. The compression punch 21 is supported by a lifting base 23 located above the die 11 via a compression spring 22. Driving means (not shown) such as a hydraulic cylinder is connected to the elevating base 23. One of the compression punches 21 can enter a gap between the inner peripheral surface of the insertion hole 14 of the die 11 and the outer peripheral surface of the cylindrical portion 17a of the punch guide 17. The other side of the cam 19 is fixed to the base 23. By moving the lifting base 23,
When the punch 18 is pressed by the cam 19, the tube body 1 inserted into the insertion hole 14 of the die 11 is simultaneously pressed by the compression punch 21 in the axial direction.

【0012】図4は、バーリング成形機30を示してい
る。バーリング成形機30は、バーリングコレット31
とテーパコーン32を有している。バーリングコレット
31とテーパコーン32は、ダイス33の成形穴33a
内に配置されている。バーリングコレット31は、先端
部が周方向に複数に分割されている。バーリングコレッ
ト31の内周面の先端部は、テーパ面31aに形成され
ている。テーパコーン32は、バーリングコレット31
の内側に配置されている。テーパコーン32には、バー
リングコレット31のテーパ面31aと摺接可能なテー
パ面32aが形成されている。バーリングコレット31
の先端部は、テーパコーン32を軸方向に移動させるこ
とにより、半径方向に変位するようになっている。
FIG. 4 shows a burring machine 30. The burring molding machine 30 has a burring collet 31.
And a taper cone 32. The burring collet 31 and the taper cone 32 are formed in the molding hole 33a of the die 33.
It is located inside. The burring collet 31 has a tip portion divided into a plurality of pieces in the circumferential direction. The tip of the inner peripheral surface of the burring collet 31 is formed into a tapered surface 31a. The taper cone 32 is a burring collet 31.
Is located inside. The taper cone 32 is formed with a taper surface 32 a capable of sliding contact with the taper surface 31 a of the burring collet 31. Burling Collet 31
The tip end portion of is moved in the radial direction by moving the taper cone 32 in the axial direction.

【0013】つぎに、本発明に係るバーリング加工方法
について説明する。図2に示すように、金属材料からな
る管体(素管)1の張り出し成形を行う前の状態では、
昇降ベース23が上昇している。この状態では、カム1
9はパンチガイド17から抜け出ており、圧縮パンチ2
1の先端もダイス11から抜け出ている。カム19およ
び圧縮パンチ21が上昇している状態では、ダイス11
の挿入穴14に管体1が挿入される。管体1がダイス1
1に挿入された状態では、管体1はダイス11とパンチ
ガイド17の間の隙間に位置することになる。
Next, the burring method according to the present invention will be described. As shown in FIG. 2, in the state before the stretch forming of the tubular body (base pipe) 1 made of a metal material,
The lift base 23 is raised. In this state, the cam 1
9 is out of the punch guide 17, and the compression punch 2
The tip of 1 also comes out of the die 11. When the cam 19 and the compression punch 21 are raised, the die 11
The tubular body 1 is inserted into the insertion hole 14 of. Tube 1 is die 1
In the state in which it is inserted in 1, the tube body 1 is located in the gap between the die 11 and the punch guide 17.

【0014】管体1のダイス11へのセットが完了する
と、上昇ベース23が下降し、カム19がパンチガイド
17の円筒部17a内に進入する。さらに、昇降ベース
23が下降すると、カム19の傾斜面19aがパンチ1
8の傾斜面18bに接触し、パンチ18はカム19の傾
斜面19aとの摺接によりダイス11の横穴15に向っ
て移動する。これと同時に、圧縮パンチ21の先端部が
ダイス11の挿入穴13に進入し、管体1が圧縮パンチ
21により軸方向に押圧される。パンチ18が横穴15
に向って移動した際には、管体1の内側がパンチ18に
よって外方に押圧される。これにより、管体1には、図
2に示すようにダイス11の横穴15とパンチ18の凸
部18aによって外方に膨出する膨出部2が形成され
る。
When the setting of the tube body 1 on the die 11 is completed, the ascending base 23 descends and the cam 19 enters into the cylindrical portion 17a of the punch guide 17. Further, when the elevating base 23 descends, the inclined surface 19a of the cam 19 causes the punch 1 to move.
8, the punch 18 moves toward the lateral hole 15 of the die 11 by sliding contact with the inclined surface 19a of the cam 19. At the same time, the tip of the compression punch 21 enters the insertion hole 13 of the die 11, and the tube 1 is pressed by the compression punch 21 in the axial direction. Punch 18 has a side hole 15
When it moves toward, the inside of the tube body 1 is pressed outward by the punch 18. As a result, as shown in FIG. 2, the tubular body 1 is formed with the bulging portion 2 bulging outward by the lateral hole 15 of the die 11 and the convex portion 18a of the punch 18.

【0015】ダイス11には、周方向に延びる拡管溝1
6が形成されているので、管体1が圧縮パンチ21によ
って軸方向に押圧された際には、管体1の一部が拡管溝
16に向けて膨出し、図2に示すように、拡径部3が形
成される。ま、変形量のバランスがとれ、管体1の中
心ずれおよび真円度ずれが防止される。
The die 11 has a pipe expanding groove 1 extending in the circumferential direction.
6 is formed, when the tube body 1 is axially pressed by the compression punch 21, a part of the tube body 1 bulges toward the tube expansion groove 16 and expands as shown in FIG. The diameter part 3 is formed . Also, the balance of the deformation amount is taken, the center deviation and circularity deviation of the tube 1 is prevented.

【0016】管体1に膨出部2と拡径部3が形成される
と、昇降ベース23が上昇し、パンチ18はリターンス
プリング20によって元の位置に戻される。つぎに、例
えばダイス11の型開きにより、管体1はパンチガイド
17から引き抜かれ、管体1の張り出し成形機10から
の取り出しが行われる。管体1が張り出し成形機10か
ら取り出されると、管体1の膨出部2の頂部には、パン
チ(図示略)によるプレス加工またはドリル(図示略)
による機械加工により、図3に示す下穴4が加工され
る。
When the bulging portion 2 and the enlarged diameter portion 3 are formed in the tubular body 1, the elevating base 23 is raised and the punch 18 is returned to its original position by the return spring 20. Next, for example, by opening the die 11, the tubular body 1 is pulled out from the punch guide 17, and the tubular body 1 is taken out from the overhang molding machine 10. When the tubular body 1 is taken out from the overhang molding machine 10, the top of the bulging portion 2 of the tubular body 1 is pressed by a punch (not shown) or drilled (not shown).
The prepared hole 4 shown in FIG. 3 is machined by the machining.

【0017】図4は、膨出部2のバーリング成形を示し
ている。管体1の膨出部2の下穴4には、バーリング成
形機30のバーリングコレット31およびテーパコーン
32が挿入される。バーリングコレット31およびテー
パコーン32を下穴4に挿入する際には、図4の中心線
の上半分に示すように、バーリングコレット31はテー
パコーン32の移動により縮径している。バーリングコ
レット31の先端部が管体1内に完全に挿入されると、
テーパコーン32の軸方向の移動により、バーリングコ
レット31は図4の中心線の下半分に示すように、下穴
4よりも大に拡径する。
FIG. 4 shows burring molding of the bulging portion 2. The burring collet 31 and the taper cone 32 of the burring molding machine 30 are inserted into the prepared hole 4 of the bulging portion 2 of the tubular body 1. When the burring collet 31 and the taper cone 32 are inserted into the pilot hole 4, the burring collet 31 is reduced in diameter by the movement of the taper cone 32 as shown in the upper half of the center line in FIG. When the tip portion of the burring collet 31 is completely inserted into the tube body 1,
Due to the axial movement of the taper cone 32, the burring collet 31 has a diameter larger than that of the prepared hole 4, as shown in the lower half of the center line in FIG.

【0018】バーリングコレット31が拡径した状態
で、バーリングコレット31およびテーパコーン32を
外方に引張ると、膨出部2がダイス33の成形穴33a
に沿って外方に延び、膨出部2はバーリングコレット3
1により下穴4が拡大されるとともに、内周面がバーリ
ングコレット31との摺接により所定の内径に仕上げら
れる。これにより、膨出部2は図5に示すようにバーリ
ング部5に成形される。
When the burring collet 31 and the taper cone 32 are pulled outward while the burring collet 31 is expanded, the bulging portion 2 causes the bulging portion 2 to be formed in the molding hole 33a of the die 33.
Extending outward along the bulge 2 and the bulge 2 is formed by the burring collet 3
1, the prepared hole 4 is enlarged, and the inner peripheral surface is finished in a predetermined inner diameter by sliding contact with the burring collet 31. As a result, the bulging portion 2 is molded into the burring portion 5 as shown in FIG.

【0019】本実施例では、管体1を、内周面に横穴1
5と拡管溝16とが形成されたダイス11に挿入し、ダ
イス11に挿入された管体1の内側に配置されるパンチ
18により管体1の内側を横穴に向けて押圧することに
より膨出部2を形成し、管体1を軸方向に押圧すること
により膨出部2と同一円周部の少なくとも一部を膨出部
2と同時に拡管溝16に向けて膨出させて拡径部3を形
成するので、液圧を用いることなく管体に膨出部2と拡
径部3を形成することが可能となる。また、膨出部2お
よび拡径部3は、パンチ18および圧縮パンチ21の押
圧によりそれぞれ形成されるので、液圧バルジ加工法に
比べて装置のシール部材の消耗等の厳密な管理が不要と
なり、加工装置を簡素化することができ、設備費の低減
およびランニングコストの低減が可能となる。また、パ
ンチによる高荷重での押圧が可能となるため、液圧バル
ジ加工法では成形困難な厚肉パイプにも、容易に適用す
ることができる。
In this embodiment, the tubular body 1 is provided with a lateral hole 1 on its inner peripheral surface.
5 and the tube expansion groove 16 are formed in the die 11, and the punch 18 arranged inside the tube body 1 inserted in the die 11 presses the inside of the tube body 1 toward the lateral hole to bulge. By forming the portion 2 and pressing the tubular body 1 in the axial direction, at least a part of the same circumferential portion as the bulging portion 2 bulges toward the pipe expanding groove 16 at the same time as the bulging portion 2 and expands the diameter. Since 3 is formed, it is possible to form the bulging portion 2 and the enlarged diameter portion 3 in the tubular body without using hydraulic pressure. Further, since the bulging portion 2 and the enlarged diameter portion 3 are formed by pressing the punch 18 and the compression punch 21, respectively, strict management such as exhaustion of the seal member of the apparatus is not necessary as compared with the hydraulic bulge processing method. Further, the processing device can be simplified, and the facility cost and the running cost can be reduced. Further, since the punch can be pressed with a high load, it can be easily applied to a thick pipe which is difficult to form by the hydraulic bulge processing method.

【0020】なお、本発明は液圧を用いて管材の一部を
膨出させる場合にも適用可能であり、膨出部の成形の際
に、膨出部に起因する管体の変形を防止することができ
る。
The present invention can also be applied to the case where a part of the pipe material is bulged by using hydraulic pressure, and when the bulging part is formed, deformation of the pipe body due to the bulging part is prevented. can do.

【0021】[0021]

【発明の効果】(1)請求項1のバーリング加工方法に
よれば、管体を、内周面に形成された横穴と内周面の横
穴と同一円周上で周方向に延び両端が横穴に接続された
拡管溝とを有するダイスに挿入し、圧縮パンチで管体を
軸方向に押圧し拡径部を形成しながらカムによりパンチ
を移動させて膨出部を形成するようにしたので、膨出部
の成形時には膨出部に起因する管体の変形を防止するこ
とができる。 (2)請求項2のバーリング加工方法によれば、管体の
真円度ずれおよび中心ずれを防止することができる。
(1) According to the burring method of the first aspect, the tubular body extends in the circumferential direction on the same circumference as the lateral hole formed in the inner peripheral surface and the lateral hole of the inner peripheral surface, and both ends are lateral holes. Connected to
Insert into a die with expansion groove and press the punch to
Punch with a cam while pressing in the axial direction to form the expanded part
Since the bulging portion is formed by moving the bulging portion, it is possible to prevent deformation of the tubular body due to the bulging portion when the bulging portion is formed. (2) According to the burring method of the second aspect, it is possible to prevent the circularity deviation and the center deviation of the tubular body.

【図面の簡単な説明】[Brief description of drawings]

【図1】本発明の一実施例に係るバーリング加工方法に
よる膨出部の成形状態を示す断面図である。
FIG. 1 is a cross-sectional view showing a molding state of a bulge portion by a burring method according to an embodiment of the present invention.

【図2】図1の方法によって成形された管体の部分拡大
断面図である。
FIG. 2 is a partially enlarged cross-sectional view of a tubular body formed by the method of FIG.

【図3】図2の管体の膨出部に下穴加工を施した状態を
示す拡大断面図である。
FIG. 3 is an enlarged cross-sectional view showing a state in which a swelled portion of the tubular body of FIG. 2 is processed into a pilot hole.

【図4】図3の管体のバーリング成形状態を示す拡大断
面図である。
FIG. 4 is an enlarged cross-sectional view showing a burring state of the tubular body of FIG.

【図5】図4のバーリング成形後における管体の部分拡
大断面図である。
5 is a partially enlarged cross-sectional view of the tubular body after the burring molding of FIG.

【符号の説明】 1 管体 2 膨出部 3 拡径部 4 下穴 5 バーリング部 10 張り出し成形機 11 ダイス 15 横穴 16 拡管溝 18 パンチ 21 圧縮パンチ 30 バーリング成形機[Explanation of symbols] 1 tube 2 bulge 3 Expanded part 4 pilot holes 5 Burling part 10 Overhang forming machine 11 dice 15 side hole 16 Expansion groove 18 punch 21 compression punch 30 Burling machine

───────────────────────────────────────────────────── フロントページの続き (56)参考文献 特開 平4−89144(JP,A) 特開 昭59−19025(JP,A) 実開 昭63−4234(JP,U) 実開 昭56−34627(JP,U) (58)調査した分野(Int.Cl.7,DB名) B21D 51/16 B21D 39/20 B21D 19/08 ─────────────────────────────────────────────────── ─── Continuation of the front page (56) Reference JP-A-4-89144 (JP, A) JP-A-59-19025 (JP, A) Actually opened 63-4234 (JP, U) Actually opened 56- 34627 (JP, U) (58) Fields surveyed (Int.Cl. 7 , DB name) B21D 51/16 B21D 39/20 B21D 19/08

Claims (2)

(57)【特許請求の範囲】(57) [Claims] 【請求項1】 管体を、内周面に形成された横穴と該横
穴と同一円周上で周方向に延び両端が前記横穴に接続さ
れた拡管溝とを有するダイスと、パンチガイドとの間に
セットする工程と、 カムと圧縮パンチを同時に下降させ、該圧縮パンチで前
記管体を軸方向に押圧し、前記管体を前記拡管溝に向け
て膨出させて拡径部を形成しながら、前記カムによりパ
ンチを移動させて前記管体を前記横穴に向けて膨出さ
せ、膨出部を形成する工程と、を有する バーリング加工
方法。
1. A tubular body is provided with a lateral hole formed on an inner peripheral surface thereof and the lateral hole.
It extends in the circumferential direction on the same circumference as the hole and both ends are connected to the lateral hole.
Between the die with the expanded pipe groove and the punch guide
At the same time as the setting process, the cam and compression punch are lowered simultaneously
The tubular body is pressed in the axial direction, and the tubular body is directed to the pipe expanding groove.
Bulge to form the expanded diameter part,
Move the punch to bulge the tube toward the lateral hole.
And a step of forming a bulge portion .
【請求項2】 前記拡管溝の断面積と前記横穴の断面積
とはほぼ等し請求項1記載のバーリング加工方法。
2. A cross-sectional area of the expansion groove and a cross-sectional area of the lateral hole.
Almost equal have claim 1 burring process according to the.
JP20073894A 1994-08-25 1994-08-25 Burring processing method Expired - Fee Related JP3394332B2 (en)