JP2001328832A - Apparatus and method for molding glass cylinder - Google Patents

Apparatus and method for molding glass cylinder

Info

Publication number
JP2001328832A
JP2001328832A JP2000145285A JP2000145285A JP2001328832A JP 2001328832 A JP2001328832 A JP 2001328832A JP 2000145285 A JP2000145285 A JP 2000145285A JP 2000145285 A JP2000145285 A JP 2000145285A JP 2001328832 A JP2001328832 A JP 2001328832A
Authority
JP
Japan
Prior art keywords
glass cylinder
jig
outer shape
glass
correcting
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP2000145285A
Other languages
Japanese (ja)
Inventor
Yuichi Kanai
裕一 金井
Tetsuya Endo
哲哉 遠藤
Yasuyuki Iwata
康幸 岩田
Takuya Adachi
拓也 足立
Kazuya Okubo
一也 大久保
Shinko Kubota
真弘 久保田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Coorstek KK
Original Assignee
Toshiba Ceramics Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toshiba Ceramics Co Ltd filed Critical Toshiba Ceramics Co Ltd
Priority to JP2000145285A priority Critical patent/JP2001328832A/en
Publication of JP2001328832A publication Critical patent/JP2001328832A/en
Pending legal-status Critical Current

Abstract

PROBLEM TO BE SOLVED: To provide an apparatus and a method for molding a glass cylinder, capable of correcting a distortion in a high accuracy, having excellent reproducibility, and capable of being automatized and operated safely. SOLUTION: This apparatus for molding a glass cylinder has a cylindrical hollow part 2s, an external form correcting jig 2 having the hollow part 2s in which a solid or a hollow glass cylinder G is rotatably stored, a rotating and driving means 3 for rotating the external form-correcting jig 2 and a heat generation means 4 for heating the glass cylinder G, heats the glass cylindrical body G while rotating the external form-correcting jig 2 and corrects the curvature of the glass cylinder G. This method is carried out by using the apparatus.

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【発明の属する技術分野】発明はガラス円柱体の成形装
置および成形方法に係わり、特にガラス円柱体の曲がり
修正を精度よく行えるガラス円柱体の成形装置および成
形方法に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to an apparatus and a method for forming a glass cylinder, and more particularly, to an apparatus and a method for forming a glass cylinder capable of accurately correcting the bending of the glass cylinder.

【0002】[0002]

【従来の技術】従来の中空の石英ガラス円柱体(石英ガ
ラス管)や中実のガラス円柱体(石英ガラス棒)などの
曲がり修正は、作業者が目視確認により修正位置を特定
し、しかる後、手でガラス円柱体の片側を持ち、これを
回転させながらバーナ炎を当てて当該部分の修正を行
い、この繰返しによって行っていた。
2. Description of the Related Art In conventional bending correction of a hollow quartz glass cylinder (quartz glass tube) or a solid glass cylinder (quartz glass rod), an operator specifies a correction position by visual confirmation, and thereafter, By holding one side of the glass cylinder by hand and rotating it, a burner flame was applied to correct the portion, and this operation was repeated.

【0003】しかし、この従来の修正方法では、複数箇
所の曲がりを同時に修正できないため、修正に時間を要
し、また、曲がり個所の確認および修正確認を目視で行
っているため、作業者によって修正された製品にバラツ
キが発生していた。さらに、作業者の手作業であるた
め、高精度の修正が困難であり、また、バーナ炎による
作業であるため、バーナを変更すると再現性が乏しく、
自動化(ライン化)が困難であり、さらに、バーナ炎の
近くで作業するため、危険であった。
However, in this conventional correction method, it is not possible to correct a plurality of bends at the same time, so that it takes time to correct the bends. Further, since the bends are checked and the corrections are visually checked, the correction is performed by an operator. The product that was used had variations. Furthermore, since it is a manual operation of an operator, it is difficult to correct with high accuracy, and since it is an operation using a burner flame, reproducibility is poor when a burner is changed,
It was difficult to automate (line) and was dangerous because it worked near burner flames.

【0004】[0004]

【発明が解決しようとする課題】そこで、曲がりを高精
度に修正でき、再現性があり、自動化が可能で、作業が
安全なガラス円柱体の成形装置および成形方法が要望さ
れていた。
Therefore, there has been a demand for a molding apparatus and a molding method of a glass cylinder which can correct the bending with high precision, has reproducibility, can be automated, and is safe in operation.

【0005】本発明は上述した事情を考慮してなされた
もので、曲がりを高精度に修正でき、再現性があり、自
動化が可能で、作業が安全なガラス円柱体の成形装置お
よび成形方法を提供することを目的とする。
The present invention has been made in view of the above-mentioned circumstances, and has an object to provide a molding apparatus and a molding method of a glass cylinder which can correct a bending with high accuracy, has reproducibility, can be automated, and is safe in operation. The purpose is to provide.

【0006】[0006]

【課題を解決するための手段】上述目的を達成するため
になされた本願請求項1の発明は、円柱形状の中空部を
有し、この中空部に中実若しくは中空のガラス円柱体が
回転自在に収納される外形修正治具と、この外形修正治
具を回転させる回転駆動手段と、前記ガラス円柱体を加
熱する発熱手段とを有し、外形修正治具を回転させなが
らガラス円柱体を加熱し、ガラス円柱体の曲がりを修正
することを特徴とするガラス円柱体の成形装置であるこ
とを要旨としている。
SUMMARY OF THE INVENTION In order to achieve the above object, the invention of claim 1 has a cylindrical hollow portion, in which a solid or hollow glass cylindrical body is rotatable. A jig accommodated in the glass, a rotation driving means for rotating the jig, and a heating means for heating the glass cylinder, and heating the glass cylinder while rotating the jig. The gist of the present invention is to provide an apparatus for forming a glass cylinder, which is characterized by correcting the bending of the glass cylinder.

【0007】本願請求項2の発明では、上記外形修正治
具は、上記中空部が設けられた円筒体であり、上記回転
駆動手段は、回転駆動される複数個の回転ローラを有
し、この回転ローラに載置された外形修正治具を回転さ
せることを特徴とする請求項1に記載のガラス円柱体の
成形装置であることを要旨としている。
In the invention of claim 2 of the present application, the outer shape correcting jig is a cylindrical body provided with the hollow portion, and the rotation driving means has a plurality of rotation rollers driven to rotate. The gist of the present invention is a glass cylinder forming apparatus according to claim 1, wherein the outer shape correcting jig placed on the rotating roller is rotated.

【0008】本願請求項3の発明では、上記外形修正治
具は、カーボンヒータ製であり、発熱手段を兼ね備えた
ことを特徴とする請求項1に記載のガラス円柱体の成形
装置であることを要旨としている。
In the invention according to claim 3 of the present invention, the outer shape correcting jig is made of a carbon heater and has a heat generating means. It is a gist.

【0009】本願請求項4の発明では、上記外形修正治
具は、複数個の加熱用透孔が穿設され、上記発熱手段は
バーナ炎であることを特徴とする請求項1または2に記
載のガラス円柱体の成形装置であることを要旨としてい
る。
In the invention of claim 4 of the present application, the outer shape correcting jig is provided with a plurality of through holes for heating, and the heating means is a burner flame. The gist of the present invention is that it is an apparatus for molding a glass cylinder.

【0010】本願請求項5の発明では、上記ガラス円柱
体は、石英ガラス製で直径が100mm以下であること
を特徴とする請求項1ないし4のいずれか1項に記載の
ガラス円柱体の成形装置であることを要旨としている。
In the invention according to claim 5 of the present application, the glass cylinder is made of quartz glass and has a diameter of 100 mm or less, and the glass cylinder according to any one of claims 1 to 4, wherein The gist is that it is a device.

【0011】本願請求項6の発明は、円筒形状の外形修
正治具に中実若しくは中空のガラス円柱体を収納して、
この外形修正治具の内周部で前記ガラス円柱体を全長に
亘って支持し、しかる後、前記ガラス円柱体を加熱した
状態で前記外形修正治具を回転し、前記ガラス円柱体を
共回りにして、前記ガラス円柱体の曲がりを修正するこ
とを特徴とするガラス円柱体の成形方法であることを要
旨としている。
According to a sixth aspect of the present invention, a solid or hollow glass cylinder is housed in a cylindrical outer shape correcting jig,
The glass cylindrical body is supported over the entire length by the inner peripheral portion of the outer shape correcting jig, and thereafter, the outer shape correcting jig is rotated while the glass cylindrical body is heated, and the glass cylindrical body is co-rotated. The gist of the present invention is a method for forming a glass cylinder, which comprises correcting the bending of the glass cylinder.

【0012】本願請求項7の発明は、中空のガラス円柱
体を、V溝を有する外形修正治具に、V溝により全長に
亘り支持するように載置し、しかる後、このガラス円柱
体に断面が円形状でガラス製の内周修正用治具を貫通
し、さらに、ガラス円柱体を加熱し、内周修正用治具に
よりガラス円柱体の曲がりを修正し、その後、ガラス円
柱体を加熱された平板形状の外形修正治具上に移載し、
ガラス円柱体を加熱しながら貫通した内周修正用治具を
下方に押付けた状態で回転して、ガラス円柱体管を共回
りにし、ガラス円柱体の外周部および内周部を修正する
ことを特徴とするガラス円柱体の成形方法であることを
要旨としている。
According to a seventh aspect of the present invention, a hollow glass cylinder is placed on an outer shape correcting jig having a V-groove so as to be supported over the entire length by the V-groove. Penetrates the glass inner circumference correction jig with a circular cross section, further heats the glass cylinder, corrects the bending of the glass cylinder with the inner circumference correction jig, and then heats the glass cylinder Transferred to the flat plate shape correction jig
Rotating the jig for fixing the inner circumference penetrated while heating the glass cylinder downward, rotating the glass cylinder body tube co-rotating, and correcting the outer circumference and inner circumference of the glass cylinder. The gist is to provide a method of forming a characteristic glass cylinder.

【0013】[0013]

【発明の実施の形態】以下、本発明に係わるガラス円柱
体の成形装置の実施形態について図面に基づき説明す
る。
DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An embodiment of a glass cylinder forming apparatus according to the present invention will be described below with reference to the drawings.

【0014】図1に示すように、本発明に係わるガラス
円柱体の成形装置1は、円柱形状の中空部2sを有し、
この中空部2sに中実ガラス円柱体(ガラス棒)若しく
は中空のガラス円柱体(ガラス管)Gが回転自在に収納
される外形修正治具2と、この外形修正治具2を回転さ
せる回転駆動手段3と、ガラス管Gを加熱する発熱手段
4とを有する。
As shown in FIG. 1, a glass cylinder forming apparatus 1 according to the present invention has a cylindrical hollow portion 2s.
An outer shape correcting jig 2 in which a solid glass cylindrical body (glass rod) or a hollow glass cylindrical body (glass tube) G is rotatably stored in the hollow portion 2s, and a rotation drive for rotating the outer shape correcting jig 2 Means 3 and heating means 4 for heating glass tube G are provided.

【0015】外形修正治具2は、外形修正治具2の中心
軸c方向に中空部2sが設けられた円筒体であり、中空
部2sに収納されたガラス管Gをその内周部2iで全長
に亘って支持し、カーボンヒータで形成され、発熱手段
4を兼ね備え、電極ブラシ5aを介して電源5に接続さ
れている。
The outer shape correction jig 2 is a cylindrical body provided with a hollow portion 2s in the direction of the central axis c of the outer shape correction jig 2, and the glass tube G housed in the hollow portion 2s is held at its inner peripheral portion 2i. It is supported over the entire length, is formed of a carbon heater, also has a heating means 4, and is connected to a power supply 5 via an electrode brush 5a.

【0016】なお、外形修正治具2は、安定した回転を
得るために円筒体であることが好ましい。
It is preferable that the outer shape correcting jig 2 is a cylindrical body in order to obtain a stable rotation.

【0017】回転駆動手段3は、図1および図2に示す
ように、基台3aに設けられた一対の支持部材3bの一
側に取付けられた回転駆動モータ3cと、この回転駆動
モータ3cにより回転される回転軸3dと、この回転軸
3dに取付けられた、例えば3対、6個の回転ローラ3
e、…、3eからなっている。従って、回転駆動モータ
3cは、複数個の回転ローラ3e、…、3e上に外形修
正治具2を載置できるようになっており、ローラ回転駆
動モータ3cを回転させることにより、回転ローラ3
e、…、3eに載置された外形修正治具2を回転させる
ことができるようになっている。
As shown in FIGS. 1 and 2, the rotation driving means 3 includes a rotation driving motor 3c attached to one side of a pair of support members 3b provided on a base 3a, and a rotation driving motor 3c. A rotating shaft 3d to be rotated and, for example, three pairs of six rotating rollers 3 attached to the rotating shaft 3d
e,..., 3e. Therefore, the rotary drive motor 3c is capable of mounting the outer shape correction jig 2 on the plurality of rotary rollers 3e,..., 3e.
,..., 3e can be rotated.

【0018】ガラス管Gは、石英ガラス製では熱膨張係
数が小さくて、加工が比較的に難しく、本発明に係わる
ガラス円柱体の成形装置は、直径が100mmを超える
ものについても、用いることができるが、直径が100
mm以下の修正が最も効果的である。
The glass tube G made of quartz glass has a small coefficient of thermal expansion and is relatively difficult to process. The apparatus for forming a glass cylinder according to the present invention can be used even if the diameter exceeds 100 mm. Yes, but with a diameter of 100
A correction of less than mm is most effective.

【0019】次にガラス円柱体の成形装置の実施形態を
用いたガラス管の曲がり修正方法について説明する。
Next, a method for correcting the bending of a glass tube using the embodiment of the apparatus for forming a glass cylinder will be described.

【0020】最初に、前工程における検査により曲がり
修正が必要なガラス管Gを、ガラス円柱体の成形装置1
の外形修正治具2に設けた中空部2sに挿入し、外形修
正治具2の内周部2iによって全長に亘って支持するよ
うに載置して、収納する。
First, a glass tube G that needs to be bent by inspection in the previous process is placed in a glass cylinder forming apparatus 1.
Is inserted into the hollow portion 2s provided in the outer shape correction jig 2, and is placed and stored so as to be supported over the entire length by the inner peripheral portion 2i of the outer shape correction jig 2.

【0021】さらに、カーボンヒータを付勢し、また、
回転駆動モータ3を付勢して、回転軸3dを介して回転
ローラ3e、…、3eを回転し、ガラス管Gを均一に軟
化するために、回転ローラ3e、…、3e上に載置した
外形修正治具2を低速回転する。そして、外形修正治具
2の低速回転に伴い、ガラス管Gも低速で回転しなが
ら、発熱手段4を兼ね備えた外形修正治具2により、ガ
ラス管G全体を均一に加熱する。
Further, the carbon heater is energized, and
.. 3e via the rotating shaft 3d by energizing the rotation drive motor 3 and placed on the rotating rollers 3e,..., 3e in order to uniformly soften the glass tube G. The outer shape correction jig 2 is rotated at a low speed. Then, with the low-speed rotation of the outer shape correction jig 2, the entire glass tube G is uniformly heated by the outer shape correction jig 2 also serving as the heating unit 4 while the glass tube G rotates at a low speed.

【0022】なお、外形修正治具2にガラス管Gを収納
したとき、熱衝撃により破損しない程度に外形修正治具
2を予熱しておけば、曲がり修正工程時間を短縮でき
る。
When the glass tube G is housed in the outer shape correction jig 2, if the outer shape correction jig 2 is preheated to the extent that it is not damaged by a thermal shock, the bending correction process time can be shortened.

【0023】しかる後、回転駆動モータ3の回転数を上
げ、回転ローラ3e、…、3e上に載置した外形修正治
具2を回転する。
Thereafter, the rotation speed of the rotation drive motor 3 is increased, and the outer shape correction jig 2 mounted on the rotation rollers 3e,.

【0024】この外形修正治具2の回転に伴い、ガラス
管Gは中空部2s内で外形修正治具2によって全長に亘
って支持した状態で回転する。この中空部2s内ので回
転により、均一に加熱し軟化しているガラス管Gを、自
重に対する反力として外形修正治具2の内周部2iから
その全長に亘って等しい力で押圧し、ガラス管Gの曲が
りを修正し、真直ぐにする。
With the rotation of the outer shape correcting jig 2, the glass tube G rotates in the hollow portion 2s while being supported over the entire length by the outer shape correcting jig 2. The glass tube G, which has been uniformly heated and softened by rotation in the hollow portion 2s, is pressed with an equal force over the entire length from the inner peripheral portion 2i of the outer shape correction jig 2 as a reaction force against its own weight. Correct the bend in tube G and straighten it.

【0025】上記曲がり修正工程において、ガラス管G
を外形修正治具2の内周部2iからその全長に亘って等
しい力で押圧するので、外形修正治具2の内周部2iに
沿って修正することができ、正確な真直度が得られ、ま
た、複数箇所の曲がりを同時に修正することが可能であ
るので、修正工程時間を短縮することができる。
In the bending correction step, the glass tube G
Is pressed from the inner peripheral portion 2i of the outer shape correction jig 2 with an equal force over the entire length thereof, so that the outer peripheral portion 2i of the outer shape correction jig 2 can be corrected, and accurate straightness can be obtained. In addition, since it is possible to simultaneously correct a plurality of bends, the time required for the correction process can be reduced.

【0026】また、外形修正治具2は、発熱手段を兼ね
備えているので、温度制御が容易であり、外形修正治具
2およびガラス管Gを均一に加熱し、その結果、再現性
のある安定した品質のガラス管Gを得ることができる。
Further, since the outer shape correcting jig 2 also has a heating means, it is easy to control the temperature, and uniformly heats the outer shape correcting jig 2 and the glass tube G. A glass tube G having a good quality can be obtained.

【0027】さらに、ガラス管Gを外形修正治具2に収
納した後は、作業者は高温の外形修正治具2に近づく必
要がないので、安全であり、また、複数箇所の曲がりを
同時に修正することが可能であるので、曲がり個所の検
知機構は不必要となり、ガラス管Gの外形修正治具2へ
の出し入れのみを考慮すればよく、自動化(ライン化)
が容易である。
Further, after the glass tube G is stored in the outer shape correction jig 2, the worker does not need to approach the high temperature outer shape correction jig 2, so it is safe, and the bending at a plurality of locations can be corrected simultaneously. Therefore, a mechanism for detecting a bent portion is not required, and only taking the glass tube G into and out of the outer shape correcting jig 2 needs to be considered.
Is easy.

【0028】次に上記実施形態の変形例を説明する。Next, a modification of the above embodiment will be described.

【0029】例えば、図3および図4に示すように、本
実施形態の変形例のガラス管の成形装置21は、円柱形
状の中空部22sを有し、この中空部22sにガラス管
Gが回転自在に収納される外形修正治具22と、この外
形修正治具22を回転させる回転駆動手段23と、ガラ
ス管Gを外部から加熱する発熱手段24とを有する。
For example, as shown in FIGS. 3 and 4, a glass tube forming apparatus 21 according to a modification of the present embodiment has a cylindrical hollow portion 22s in which the glass tube G is rotated. It has an outer shape correcting jig 22 that can be freely stored, a rotation driving unit 23 that rotates the outer shape correcting jig 22, and a heat generating unit 24 that heats the glass tube G from outside.

【0030】上記外形修正治具22は、外形修正治具2
2の中心軸c方向に中空部22Sが設けられたカーボン
製の円筒体であり、複数個の加熱用透孔22a、22
a、…、22aが穿設されている。外形修正治具22は
軸支して回転させる場合には、中空部が円柱形状であれ
ば、外周断面が円形状である必要はなく、多角形等であ
ってもよい。
The outer shape correcting jig 22 includes the outer shape correcting jig 2
2 is a carbon cylindrical body provided with a hollow portion 22S in the direction of the central axis c, and a plurality of heating through holes 22a, 22
, 22a are bored. When the outer shape correction jig 22 is pivotally supported and rotated, as long as the hollow portion has a columnar shape, the outer peripheral cross-section does not need to be circular but may be polygonal or the like.

【0031】また、発熱手段24は、外形修正治具22
に対向する下方に配置された酸水素バーナ24a、24
a、24aで発生するバーナ炎であり、外形修正治具2
2を加熱することにより、間接的にガラス管Gを加熱
し、加熱用透孔22a、22a、…、22aを介して、
酸水素バーナ24a、24a、24aからのバーナ炎に
より、直接ガラス管Gを加熱するようになっている。
The heat generating means 24 includes the outer shape correcting jig 22.
Oxyhydrogen burners 24a, 24 disposed below and facing
a, a burner flame generated at 24a, and an outer shape correction jig 2
2 is heated indirectly to heat the glass tube G, and through the heating through holes 22a, 22a,.
The glass tube G is directly heated by the burner flame from the oxyhydrogen burners 24a, 24a, 24a.

【0032】さらに、回転駆動手段23は、上記実施形
態と同様に図3および図4に示すように、基台23a、
支持部材23bの一側に取付けられた回転駆動モータ2
3cと、回転軸23dに取付けられた、回転ローラ23
e、…、23eからなっている。
Further, as shown in FIGS. 3 and 4, the rotation driving means 23 includes a base 23a,
Rotary drive motor 2 mounted on one side of support member 23b
3c and a rotating roller 23 attached to a rotating shaft 23d.
,..., 23e.

【0033】次に上記本変形例を用いたガラス管の曲が
りを修正する方法について説明する。
Next, a description will be given of a method of correcting the bending of the glass tube using the above-described modified example.

【0034】曲がり修正が必要なガラス管Gを、外形修
正治具22の中空部22sに挿入し、外形修正治具22
によって全長に亘って支持するように載置して、収納す
る。
The glass tube G that needs to be bent is inserted into the hollow portion 22s of the outer shape correction jig 22, and the outer shape correction jig 22 is inserted.
And are stored so as to be supported over the entire length.

【0035】しかる後、酸水素バーナ24a、24a、
…、24aを点火してバーナ炎を発生させ、さらに、回
転駆動モータ23cを付勢して、回転ローラ23e、
…、23eを回転し、ガラス管Gを均一に軟化するよう
に、回転ローラ23e、…、23e上に載置した外形修
正治具22を低速回転する。
Thereafter, the oxyhydrogen burners 24a, 24a,
, 24a are ignited to generate a burner flame, and furthermore, the rotary drive motor 23c is urged to rotate the rotary rollers 23e,
, 23e are rotated, and the outer shape correcting jig 22 placed on the rotating rollers 23e, ..., 23e is rotated at a low speed so that the glass tube G is softened uniformly.

【0036】ガラス管Gをバーナ炎により加熱した外形
修正治具22から間接的に加熱し、さらに、バーナ炎か
らの熱を、加熱用透孔22a、22a、…、22aを介
して直接受けて加熱し、軟化する。
The glass tube G is indirectly heated from the outer shape correcting jig 22 heated by the burner flame, and further receives the heat from the burner flame directly through the heating through holes 22a, 22a,. Heat and soften.

【0037】しかる後、回転駆動モータ23の回転数を
上げ、回転ローラ23e、…、23e上に載置した外形
修正治具22を回転する。
Thereafter, the rotation speed of the rotation drive motor 23 is increased, and the outer shape correction jig 22 mounted on the rotation rollers 23e,..., 23e is rotated.

【0038】この外形修正治具22の回転に伴い、ガラ
ス管Gを中空部22s内で外形修正治具22によって全
長に亘って支持した状態で共回りに回転する。この中空
部22s内での回転により、均一に加熱し軟化している
ガラス管Gを、自重に対する反力として外形修正治具2
2の内周部22iからその全長に亘って等しい力で押圧
し、ガラス管Gの曲がりを修正して、真直ぐにする。
With the rotation of the outer shape correcting jig 22, the glass tube G rotates co-rotating in the hollow portion 22s while being supported over the entire length by the outer shape correcting jig 22. The glass tube G, which has been uniformly heated and softened by the rotation in the hollow portion 22s, is turned into a reaction force against its own weight, and the outer shape correction jig 2 is used.
2 is pressed from the inner peripheral portion 22i with the same force over the entire length to correct the bending of the glass tube G and straighten it.

【0039】上記変形例を用いた曲がり修正工程におい
て、上述した実施形態と同様に、ガラス管Gを、外形修
正治具22の内周部22iに沿って修正し、正確な真直
度が得られ、また、複数箇所の曲がりを同時に修正する
ことが可能であるので、修正工程時間を短縮することが
でき、さらに、作業者は高温の外形修正治具2に近づく
必要がないので、安全であり、また、自動化(ライン
化)が容易である。
In the bending correction process using the above-described modification, the glass tube G is corrected along the inner peripheral portion 22i of the outer shape correction jig 22 in the same manner as in the above-described embodiment, and accurate straightness can be obtained. In addition, since it is possible to correct the bending at a plurality of locations at the same time, the time required for the correction process can be shortened. Further, since the operator does not need to approach the high-temperature outer shape correction jig 2, it is safe. Also, automation (line conversion) is easy.

【0040】さらに、外形修正治具22を加熱すること
により、間接的にガラス管Gを加熱し、かつ、加熱用透
孔22a、22a、…、22aを介して、酸水素バーナ
24a、24a、24aからのバーナ炎により、直接ガ
ラス管Gを加熱するので、修正時間を短縮できる。
Further, by heating the outer shape correction jig 22, the glass tube G is indirectly heated, and the oxyhydrogen burners 24a, 24a, 24a, 24a,. Since the glass tube G is directly heated by the burner flame from 24a, the correction time can be reduced.

【0041】次に本発明に係わるガラス円柱体の成形方
法の実施形態について図面に基づき説明する。
Next, an embodiment of a method for forming a glass cylinder according to the present invention will be described with reference to the drawings.

【0042】図5(a)、(b)に示すように、本発明
に係わるガラス円柱体の成形方法の実施形態に用いられ
るガラス管の成形装置41は、ガラス管Gが載置される
外形修正治具42と、この外形修正治具42に載置され
たガラス管Gを貫通する内周修正治具43と、この内周
修正治具43を回転させる内周修正治具回転機構44
と、上記成形装置41に近接して配置される平板修正治
具45とを有している。
As shown in FIGS. 5A and 5B, the glass tube forming apparatus 41 used in the embodiment of the glass column forming method according to the present invention has an outer shape on which the glass tube G is mounted. A correction jig 42, an inner circumference correction jig 43 that penetrates the glass tube G placed on the outer shape correction jig 42, and an inner circumference correction jig rotating mechanism 44 that rotates the inner circumference correction jig 43.
And a flat plate correction jig 45 arranged close to the molding device 41.

【0043】上記外形修正治具42は、カーボンヒータ
製で、発熱手段を兼ね備え、電源46に接続され、ガラ
ス管Gが全長に亘って支持されるように載置されるV溝
42aが形成されている。
The outer shape correcting jig 42 is made of a carbon heater, has a heating means, is connected to a power supply 46, and has a V-shaped groove 42a on which the glass tube G is mounted so as to be supported over its entire length. ing.

【0044】さらに、内周修正治具43は、ガラスGを
貫通し、石英ガラス製、長尺円柱体形状をなし、図6に
示すように、設置位置が移動可能に設けられた後述する
内周修正治具回転駆動機構44の回転ローラ44a、4
4a、44bおよび回転ローラ44c、44c、44d
により着脱自在に橋設され、さらに、石英ガラス管43
aにカーボンヒータ43bを嵌合して形成され、電源
(図示せず)により付勢され、修正されるガラス管Gを
内周から加熱できるようになっている。
Further, the inner circumference correcting jig 43 penetrates the glass G, is made of quartz glass, has a long cylindrical shape, and has an inner position which will be described later, as shown in FIG. The rotation rollers 44a, 4 of the circumference correction jig rotation drive mechanism 44
4a, 44b and rotating rollers 44c, 44c, 44d
Is detachably bridged by a quartz glass tube 43.
The glass tube G is formed by fitting a carbon heater 43b to a, and is urged by a power supply (not shown) so that the glass tube G to be modified can be heated from the inner periphery.

【0045】なお、内周修正治具43は必ずしもカーボ
ンヒータ43bを設ける必要はないが、カーボンヒータ
43bを付勢し、ガラス管Gを内周から加熱できること
により加熱速度を向上させることができる。
Although the inner peripheral correction jig 43 does not necessarily need to be provided with the carbon heater 43b, the heating speed can be improved by energizing the carbon heater 43b and heating the glass tube G from the inner periphery.

【0046】上記内周修正治具回転機構44は、山形三
角形状に配置された3個一組の回転駆動ローラ44a、
44a、44bからなり、三角形の頂点の位置に配置さ
れた回転駆動ローラ44bは、駆動モータ44mによっ
て回転されるようになっており、さらに、適宜位置を変
え、回転駆動ローラ44a、44a間に内周修正治具4
3を載置あるいは、取り去ることができるようになって
いる。また、外形修正治具42を挟んでもう一組の回転
駆動ローラ44c、44c、44dが設けられている。
但し、回転駆動ローラ44dは適宜位置を変えることが
できるが、駆動モータは取付けられていない。
The inner circumference correcting jig rotating mechanism 44 includes a set of three rotating drive rollers 44a arranged in a mountain triangular shape.
The rotary drive roller 44b, which is composed of the rotary drive rollers 44a and 44b, is disposed at the position of the vertex of the triangle and is rotated by the drive motor 44m. Circumference correction jig 4
3 can be placed or removed. Further, another pair of rotation drive rollers 44c, 44c, and 44d are provided with the outer shape correction jig 42 interposed therebetween.
However, the position of the rotary drive roller 44d can be changed as appropriate, but no drive motor is attached.

【0047】また、平板修正治具45は、カーボンヒー
タ製で、発熱手段を兼ね備え、電源47に接続され、上
面45aでガラス管Gが全長に亘って支持されるように
載置されるようになっている。
The flat plate correcting jig 45 is made of a carbon heater, has a heating means, is connected to a power supply 47, and is mounted so that the glass tube G is supported over the entire length on the upper surface 45a. Has become.

【0048】また、図5(a)示すように、外形修正治
具42の上方には、酸水素バーナ48が配置され、図5
(b)に示すように、平板修正治具45の上方には、酸
水素バーナ49が配置されている。
As shown in FIG. 5A, an oxyhydrogen burner 48 is disposed above the outer shape correction jig 42.
As shown in (b), an oxyhydrogen burner 49 is arranged above the flat plate correction jig 45.

【0049】次に上記ガラス円柱体の成形方法の実施形
態について説明する。
Next, an embodiment of the method for forming a glass cylinder will be described.

【0050】図5(a)に示すように、最初に、曲がり
修正が必要なガラス管Gを、V溝42aで全長に亘って
支持しながら、外形修正治具42に載置する。
As shown in FIG. 5 (a), first, a glass tube G requiring bending correction is placed on an outer shape correction jig 42 while being supported over the entire length by a V-groove 42a.

【0051】次にガラス管Gに内周修正治具43を貫通
し、潰れを防止した後、電源46をオンにて外形修正治
具42を発熱、加熱し、また、酸水素バーナ48を点火
してバーナ炎を発生させ、このバーナ炎および外形修正
治具42により、ガラス管Gを加熱して軟化する。その
後、内周修正治具回転駆動機構44を動作して、ガラス
管GをV溝42a内でゆっくり数回転し、ガラス管Gの
自重に対するV溝42aからの反力でガラス管Gの曲が
りを修正する。
Next, after penetrating the inner circumference correction jig 43 into the glass tube G to prevent the jig 43 from being crushed, the power supply 46 is turned on to heat and heat the outer shape correction jig 42, and the oxyhydrogen burner 48 is ignited. Then, a burner flame is generated, and the glass tube G is heated and softened by the burner flame and the outer shape correcting jig 42. Thereafter, the inner circumference correcting jig rotation drive mechanism 44 is operated to rotate the glass tube G several times slowly in the V-groove 42a, and the glass tube G is bent by a reaction force from the V-groove 42a with respect to its own weight. Fix it.

【0052】さらに、内周修正治具43により、ガラス
管Gを全長に亘り平板修正治具45に押圧し、内周修正
治具回転駆動機構44の作用で内周修正治具43を回転
して、この内周修正治具43の回転に伴ってガラス管G
を共回りにして、内周部および外周部の修正を行う。
Further, the glass tube G is pressed against the flat plate correcting jig 45 over the entire length by the inner peripheral correcting jig 43, and the inner peripheral correcting jig 43 is rotated by the operation of the inner peripheral correcting jig rotation drive mechanism 44. With the rotation of the inner circumference correction jig 43, the glass tube G
Are rotated around, and the inner and outer peripheral portions are corrected.

【0053】しかる後、図5(b)に示すように、内周
修正治具43を貫通したままの状態で、上記成形装置4
1に近接して配置され、加熱状態にある平板修正治具4
5上の上面45a上に移載する。さらに平板修正治具4
5、酸水素バーナ49および電源47により付勢したカ
ーボンヒータ43aにより、ガラス管Gを外部および内
部から加熱する。
Thereafter, as shown in FIG. 5 (b), the molding device 4 is kept in a state where the inner peripheral correction jig 43 is pierced.
A flat plate correction jig 4 which is arranged close to 1 and is in a heated state
5 on the upper surface 45a. Furthermore, flat plate correction jig 4
5. The glass tube G is externally and internally heated by the oxyhydrogen burner 49 and the carbon heater 43a energized by the power supply 47.

【0054】上記のように、曲がり修正工程において
は、ガラス管Gを外形修正治具43のV溝43aからそ
の全長に亘って等しい力で押圧するので、外形修正治具
43のV溝43aに沿って修正し、正確な真直度にで
き、また、複数箇所の曲がりを同時に修正することが可
能であるので、修正工程時間を短縮することができる。
As described above, in the bending correction step, the glass tube G is pressed from the V groove 43a of the outer shape correction jig 43 with the same force over the entire length thereof. Therefore, it is possible to correct the straightness accurately and to correct the bending at a plurality of places at the same time, so that the time required for the correction process can be reduced.

【0055】さらに、平板修正治具45上での修正で
は、この内周修正治具43の回転に伴ってガラス管Gを
上面5a上で共回りにするので、内周部および外周部の
凹凸なども同時に内外周の両断面を円形に修正すること
ができる。
Further, in the correction on the flat plate correction jig 45, the glass tube G rotates coaxially on the upper surface 5a with the rotation of the inner circumference correction jig 43. In addition, both cross sections of the inner and outer peripheries can be simultaneously modified to be circular.

【0056】[0056]

【発明の効果】本発明に係わるガラス円柱体管の成形装
置および成形方法によれば、曲がりを高精度に修正で
き、再現性があり、自動化が可能で、作業が安全なガラ
ス円柱体の成形装置および成形方法を提供することがで
きる。
According to the apparatus and method for forming a glass cylinder tube according to the present invention, the bending can be corrected with high accuracy, the reproducibility is high, the automation is possible, and the molding of the glass cylinder is safe. An apparatus and a molding method can be provided.

【0057】すなわち、円柱形状の中空部を有し、この
中空部に中実若しくは中空のガラス円柱体が回転自在に
収納される外形修正治具と、この外形修正治具を回転さ
せる回転駆動手段と、ガラス円柱体を加熱する発熱手段
とを有し、外形修正治具を回転させながらガラス円柱体
を加熱し、ガラス円柱体の曲がりを修正するガラス円柱
体の成形装置であるので、ガラス円柱体を外形修正治具
の内周部からその全長に亘って等しい力で押圧して、外
形修正治具の内周部に沿って修正し、正確な真直度を得
ることができ、また、複数箇所の曲がりを同時に修正す
ることが可能であり、修正工程時間を短縮することがで
きる。さらに、ガラス円柱体を外形修正治具に収納した
後は、作業者は高温の外形修正治具に近づく必要がな
く、安全であり、また、曲がり個所の検知機構は不必要
となり、ガラス円柱体の外形修正治具への出し入れのみ
を考慮すればよく、自動化(ライン化)が容易である。
That is, an outer shape correcting jig having a cylindrical hollow portion, in which a solid or hollow glass cylindrical body is rotatably housed, and a rotation driving means for rotating the outer shape correcting jig And a heating means for heating the glass cylinder, and a glass cylinder forming apparatus for heating the glass cylinder while rotating the outer shape correction jig and correcting the bending of the glass cylinder. The body is pressed from the inner peripheral portion of the outer shape correcting jig with an equal force over the entire length thereof, and is corrected along the inner peripheral portion of the outer shape correcting jig to obtain an accurate straightness. It is possible to correct the bending of a portion at the same time, and it is possible to shorten the correction process time. Furthermore, after the glass cylinder is stored in the outer shape correction jig, the worker does not need to approach the high temperature outer shape correction jig, is safe, and the mechanism for detecting a bent portion is unnecessary. It is only necessary to consider the taking in and out of the outer shape correction jig, and automation (line formation) is easy.

【0058】また、外形修正治具は、中空部が設けられ
た円筒体であり、回転駆動手段は、回転駆動される複数
個の回転ローラを有し、この回転ローラに載置された外
形修正治具を回転させるので、簡易な機構で外形修正治
具を正確に水平回転することができ、ガラス円柱体を水
平回転し、正確な真直度を得ることができる。
Further, the outer shape correcting jig is a cylindrical body having a hollow portion, and the rotation driving means has a plurality of rotary rollers driven to rotate, and the outer shape correcting jig mounted on the rotary rollers. Since the jig is rotated, the outline correction jig can be accurately and horizontally rotated by a simple mechanism, and the glass cylinder can be horizontally rotated to obtain accurate straightness.

【0059】また、外形修正治具は、カーボンヒータ製
であり、発熱手段を兼ね備えているので、温度制御が容
易であり、外形修正治具およびガラス円柱体を均一に加
熱でき、その結果、再現性のある安定した品質のガラス
円柱体を得ることができる。
Further, since the outer shape correction jig is made of a carbon heater and also has a heating means, temperature control is easy, and the outer shape correction jig and the glass cylinder can be uniformly heated. It is possible to obtain a reliable and stable quality glass cylinder.

【0060】また、外形修正治具は、複数個の加熱用透
孔が穿設され、発熱手段はバーナ炎であるので、外形修
正治具を介して間接的にガラス円柱体を加熱し、かつ、
加熱用透孔を介して、バーナ炎により、直接ガラス円柱
体を加熱することができ、修正時間を短縮できる。
Further, since the outer shape correcting jig has a plurality of heating through holes and the heating means is a burner flame, the glass column is indirectly heated via the outer shape correcting jig, and ,
The glass cylinder can be directly heated by the burner flame through the heating through hole, and the correction time can be reduced.

【0061】また、円筒形状の外形修正治具に中実若し
くは中空のガラス円柱体を収納して、この外形修正治具
の内周部でガラス円柱体を全長に亘って支持し、しかる
後、ガラス円柱体を加熱した状態で外形修正を回転し、
ガラス円柱体を共回りにして、ガラス円柱体の曲がりを
修正するガラス円柱体の成形方法であるので、外形修正
治具の内周部に沿って修正し、正確な真直度を得ること
ができ、また、複数箇所の曲がりを同時に修正すること
が可能であり、修正工程時間を短縮することができる。
作業者は高温の外形修正治具に近づく必要がなく、安全
であり、また、曲がり個所の検知機構は不必要となり、
ガラス円柱体の外形修正治具への出し入れのみを考慮す
ればよく、ラインへ組み込んで採用することが可能であ
る。
Further, a solid or hollow glass cylinder is accommodated in a cylindrical outer shape correcting jig, and the glass cylindrical body is supported over the entire length by the inner peripheral portion of the outer shape correcting jig. Rotate the outer shape correction while heating the glass cylinder,
Since the method is a glass cylinder molding method that corrects the bending of the glass cylinder by making the glass cylinder co-rotate, it can be corrected along the inner periphery of the outer shape correction jig to obtain accurate straightness. Further, it is possible to correct the bending at a plurality of places at the same time, and it is possible to shorten the time required for the correction process.
The worker does not need to approach the hot external shape correction jig, it is safe, and the detection mechanism of the bend is unnecessary,
It is only necessary to consider taking the glass cylinder into and out of the outer shape correction jig, and it is possible to incorporate the glass cylinder into the line and adopt it.

【0062】また、中空のガラス円柱体を、V溝を有す
る外形修正治具に、V溝により全長に亘り支持するよう
に載置し、しかる後、このガラス円柱体に断面が円形状
でガラス製の内周修正用治具を貫通し、さらに、ガラス
円柱体を加熱し、内周修正用治具によりガラス円柱体の
曲がりを修正し、その後、ガラス円柱体を加熱された平
板形状の外形修正治具上に移載し、ガラス円柱体を加熱
しながら貫通した内周修正用治具を下方に押付けた状態
で回転して、ガラス円柱体を共回りにし、ガラス円柱体
の外周部および内周部を修正するガラス円柱体の成形方
法であるので、ガラス円柱体(ガラス管)を外形修正治
具のV溝からその全長に亘って等しい力で押圧し、外形
修正治具のV溝に沿って修正し、正確な真直度が得ら
れ、また、複数箇所の曲がりを同時に修正することが可
能となり、修正工程時間を短縮することができる。さら
に、内周修正治具の回転に伴ってガラス円柱体を共回り
にするので、内周部および外周部の凹凸なども同時に修
正することができる。
Further, the hollow glass cylinder is placed on an outer shape correcting jig having a V-groove so as to be supported over the entire length by the V-groove. Thereafter, the glass cylinder has a circular cross-section. Through the jig for fixing the inner circumference made of aluminum, further heats the glass cylinder, corrects the bending of the glass cylinder with the jig for correcting the inner circumference, and then heats the glass cylinder to a flat outer shape Transferred onto the correction jig, rotating while holding down the inner circumference correction jig that penetrated while heating the glass cylinder, making the glass cylinder co-rotate, the outer periphery of the glass cylinder and Since the method is a method of forming a glass cylinder for correcting the inner peripheral portion, the glass cylinder (glass tube) is pressed from the V-groove of the outer shape correcting jig with an equal force over the entire length thereof, and the V-groove of the outer shape correcting jig is pressed. To correct straightness, and Bend it is possible to modify simultaneously, it is possible to shorten the correction step time. Furthermore, since the glass cylinder rotates co-rotatively with the rotation of the inner circumference correcting jig, the unevenness of the inner circumferential portion and the outer circumferential portion can be corrected at the same time.

【図面の簡単な説明】[Brief description of the drawings]

【図1】本発明に係わるガラス円柱体の成形装置の一部
を断面にして示す側面図。
FIG. 1 is a side view showing a cross section of a part of a glass cylinder forming apparatus according to the present invention.

【図2】図1に示す本発明に係わるガラス円柱体の成形
装置のA−A線に沿う断面図。
FIG. 2 is a sectional view taken along line AA of the apparatus for forming a glass cylinder according to the present invention shown in FIG.

【図3】本発明に係わるガラス円柱体の成形装置の変形
例の一部を断面にして示す側面図。
FIG. 3 is a side view showing, in section, a part of a modification of the glass cylinder forming apparatus according to the present invention.

【図4】図3に示す本発明に係わるガラス円柱体の成形
装置の変形例のB−B線に沿う断面図。
FIG. 4 is a cross-sectional view taken along the line BB of a modification of the apparatus for forming a glass cylinder according to the present invention shown in FIG.

【図5】図5(a)、(b)は、本発明に係わるの円柱
体の成形方法に用いられるガラス円柱体の成形装置の概
略図。
FIGS. 5A and 5B are schematic views of a glass column forming apparatus used in the column forming method according to the present invention.

【図6】本発明に係わるガラス円柱体の成形方法に用い
られる内周修正治具の概略図。
FIG. 6 is a schematic view of an inner circumference correcting jig used in the method of forming a glass cylinder according to the present invention.

【符号の説明】[Explanation of symbols]

1 ガラス円柱体の成形装置 2 外形修正治具 2i 内周部 2s 中空部 3 回転駆動手段 3a 基台 3b 支持部材 3c 回転駆動モータ 3d 回転軸 3e 回転ローラ 4 発熱手段 5 電源 5a 電極ブラシ 21 ガラス円柱体の成形装置 22s 中空部 22 外形修正治具 23 回転駆動手段 24 発熱手段 22a 加熱用透孔 25 回転駆動手段 25a 基台 25b 支持部材 25c 回転駆動モータ 25d 回転軸 25e 回転ローラ 41 ガラス円柱体の成形装置 42 V溝外形修正治具 42a V溝 43 内周修正治具 43a 石英ガラス管 43b カーボンヒータ 44 内周修正治具回転機構 44a 回転ローラ 44b 回転ローラ 44c 回転ローラ 44d 回転ローラ 44m 駆動モータ 45 平板修正治具 45a 上面 46 電源 47 電源 48 酸水素バーナ 49 酸水素バーナ c 中心軸 G ガラス円柱体(ガラス管) DESCRIPTION OF SYMBOLS 1 Forming apparatus of a glass cylinder 2 Shape correction jig 2i Inner peripheral part 2s hollow part 3 Rotation drive means 3a Base 3b Support member 3c Rotation drive motor 3d Rotation shaft 3e Rotation roller 4 Heat generation means 5 Power supply 5a Electrode brush 21 Glass cylinder Body forming device 22s Hollow portion 22 Outer shape correction jig 23 Rotation driving means 24 Heat generation means 22a Heating hole 25 Rotation driving means 25a Base 25b Support member 25c Rotation driving motor 25d Rotation shaft 25e Rotation roller 41 Molding glass cylinder Apparatus 42 V groove outer shape correction jig 42a V groove 43 inner circumference correction jig 43a quartz glass tube 43b carbon heater 44 inner circumference correction jig rotation mechanism 44a rotation roller 44b rotation roller 44c rotation roller 44d rotation roller 44m drive motor 45 flat plate correction Jig 45a Upper surface 46 Power supply 47 Power supply 48 Hydrogen burner 49 oxyhydrogen burner c central axis G glass cylindrical member (glass tube)

フロントページの続き (72)発明者 岩田 康幸 愛知県刈谷市小垣江町南藤1番地 東芝セ ラミックス株式会社刈谷製造所内 (72)発明者 足立 拓也 神奈川県秦野市曽屋30番地 東芝セラミッ クス株式会社開発研究所内 (72)発明者 大久保 一也 神奈川県秦野市曽屋30番地 東芝セラミッ クス株式会社開発研究所内 (72)発明者 久保田 真弘 神奈川県秦野市曽屋30番地 東芝セラミッ クス株式会社開発研究所内 Fターム(参考) 4G014 AH00 4G015 BA08 BA09 BB01 BB03 Continued on the front page (72) Inventor Yasuyuki Iwata 1 Minamifuji, Ogakie-cho, Kariya-shi, Aichi Prefecture Toshiba Ceramics Co., Ltd.Kariya Works (72) Inventor Takuya Adachi 30 Soya, Hadano-shi, Kanagawa Prefecture Toshiba Ceramics Corporation In-house (72) Inventor Kazuya Okubo 30 Soya, Hadano-shi, Kanagawa Toshiba Ceramics Co., Ltd. (72) Inventor Mahiro Kubota 30 Soya, Hadano-shi, Kanagawa F-term in Toshiba Ceramics Co., Ltd. ) 4G014 AH00 4G015 BA08 BA09 BB01 BB03

Claims (7)

【特許請求の範囲】[Claims] 【請求項1】 円柱形状の中空部を有し、この中空部に
中実若しくは中空のガラス円柱体が回転自在に収納され
る外形修正治具と、この外形修正治具を回転させる回転
駆動手段と、前記ガラス円柱体を加熱する発熱手段とを
有し、外形修正治具を回転させながらガラス円柱体を加
熱し、ガラス円柱体の曲がりを修正することを特徴とす
るガラス円柱体の成形装置。
1. An outer shape correcting jig having a cylindrical hollow portion, in which a solid or hollow glass cylindrical body is rotatably housed, and a rotation drive means for rotating the outer shape correcting jig. And a heating means for heating the glass cylinder, heating the glass cylinder while rotating the outer shape correction jig, and correcting the bending of the glass cylinder, wherein the molding apparatus for the glass cylinder is formed. .
【請求項2】 上記外形修正治具は、上記中空部が設け
られた円筒体であり、上記回転駆動手段は、回転駆動さ
れる複数個の回転ローラを有し、この回転ローラに載置
された外形修正治具を回転させることを特徴とする請求
項1に記載のガラス円柱体の成形装置。
2. The outer shape correction jig is a cylindrical body provided with the hollow portion, and the rotation driving means has a plurality of rotation rollers driven to rotate, and is mounted on the rotation rollers. The apparatus for forming a glass cylinder according to claim 1, wherein the jig is rotated.
【請求項3】 上記外形修正治具は、カーボンヒータ製
であり、発熱手段を兼ね備えたことを特徴とする請求項
1に記載のガラス円柱体の成形装置。
3. The apparatus according to claim 1, wherein the outer shape correction jig is made of a carbon heater, and has a heat generating means.
【請求項4】 上記外形修正治具は、複数個の加熱用透
孔が穿設され、上記発熱手段はバーナ炎であることを特
徴とする請求項1または2に記載のガラス円柱体の成形
装置。
4. The molding of a glass cylinder according to claim 1, wherein the outer shape correcting jig has a plurality of through holes for heating, and the heating means is a burner flame. apparatus.
【請求項5】 上記ガラス円柱体は、石英ガラス製で直
径が100mm以下であることを特徴とする請求項1な
いし4のいずれか1項に記載のガラス円柱体の成形装
置。
5. The apparatus according to claim 1, wherein the glass cylinder is made of quartz glass and has a diameter of 100 mm or less.
【請求項6】 円筒形状の外形修正治具に中実若しくは
中空のガラス円柱体を収納して、この外形修正治具の内
周部で前記ガラス円柱体を全長に亘って支持し、しかる
後、前記ガラス円柱体を加熱した状態で前記外形修正治
具を回転し、前記ガラス円柱体を共回りにして、前記ガ
ラス円柱体の曲がりを修正することを特徴とするガラス
円柱体の成形方法。
6. A solid or hollow glass cylinder is housed in a cylindrical shape correcting jig, and the glass cylindrical body is supported over the entire length by an inner peripheral portion of the shape correcting jig. A method of forming a glass cylinder, comprising: rotating the outer shape correction jig while heating the glass cylinder to make the glass cylinder co-rotate to correct the bending of the glass cylinder.
【請求項7】 中空のガラス円柱体を、V溝を有する外
形修正治具に、V溝により全長に亘り支持するように載
置し、しかる後、このガラス円柱体に断面が円形状でガ
ラス製の内周修正用治具を貫通し、さらに、ガラス円柱
体を加熱し、内周修正用治具によりガラス円柱体の曲が
りを修正し、その後、ガラス円柱体を加熱された平板形
状の外形修正治具上に移載し、ガラス円柱体を加熱しな
がら貫通した内周修正用治具を下方に押付けた状態で回
転して、ガラス円柱体を共回りにし、ガラス円柱体の外
周部および内周部を修正することを特徴とするガラス円
柱体の成形方法。
7. A hollow glass cylinder is placed on an outer shape correcting jig having a V-groove so as to be supported by the V-groove over its entire length. Thereafter, the glass cylinder has a circular cross-section. Through the jig for fixing the inner circumference made of aluminum, further heats the glass cylinder, corrects the bending of the glass cylinder with the jig for correcting the inner circumference, and then heats the glass cylinder to a flat outer shape Transferred onto the correction jig, rotating while holding down the inner circumference correction jig that penetrated while heating the glass cylinder, making the glass cylinder co-rotate, the outer periphery of the glass cylinder and A method of forming a glass cylinder, wherein an inner peripheral portion is corrected.
JP2000145285A 2000-05-17 2000-05-17 Apparatus and method for molding glass cylinder Pending JP2001328832A (en)