IE42764B1 - Nontacky coating and adhesive compositions - Google Patents

Nontacky coating and adhesive compositions

Info

Publication number
IE42764B1
IE42764B1 IE282575A IE282575A IE42764B1 IE 42764 B1 IE42764 B1 IE 42764B1 IE 282575 A IE282575 A IE 282575A IE 282575 A IE282575 A IE 282575A IE 42764 B1 IE42764 B1 IE 42764B1
Authority
IE
Ireland
Prior art keywords
composition
solvent
anaerobically curable
initiator
organic
Prior art date
Application number
IE282575A
Original Assignee
Loctite Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Loctite Ltd filed Critical Loctite Ltd
Priority to IE282575A priority Critical patent/IE42764B1/en
Publication of IE42764B1 publication Critical patent/IE42764B1/en

Description

This invention relates to nontacky coating and adhesive compositions.
Free radical curing compositions based on acrylate-type monomers, such as methylmethacrylate, among others, have long been known. Such compositions are typically initiated by organic peroxy compounds, e.g., benzoyl peroxide and methylethyl ketone peroxide, or by radiation-activated free radical generators such as benzophenone in combination with UV light. It has also been recognized that cure of such acrylate-type compositions is often inhibited to some extent by contact with oxygen, Such as in atmospheric air. While this undesirable inhibiting effect can be overcome by various means, such as by application of heat, the need for surface curing at room temperature has not always been met. To facilitate handling, > it is often desirable to obtain a dry-to-the-touoh surface on the adhesive or coating even before any substantial cure has been effected.
More recently, the oxygen inhibition effect has been developed and commercially exploited in certain anaerobic I curing adhesives and sealants. These compositions depend on the exclusion of oxygen from the composition to allow curing to take place, usually between nonporous surfaces, as in threaded joints. These compositions remain liquid.when in contact with an adequate concentration of oxygen, such as occurs in the atmosphere. In practice, this means that the compositions can be stored for long periods in thin-walled polyethylene containers or in the aerosol-type dispensers prepared as described in U. S. Patent 3,736,260. Examples of li i these anaerobic compositions have been described in detail in U. S. Patents 2,895,950; 3,218,305; 3,425,988; and 3,435,012, among others, as well as British Specification 1,412,940. The compositions depend on the generation of free radicals, nor5 mally by a redox-type reaction catalyzed by the metallic surfaces to which the compositions are applied in use, or by pre-applied primers. It has also been found that some of these compositions can be cured by exposing them to nonionizing radiation, such as UV light; this is disclosed in French Patent 73.17729.
An anaerobic composition has as required elements a free radical polymerizable monomer (normally a mono-, di- or triacrylate or methacrylate) and a peroxy initiator or a photoinitiator, or both. It may include accelerators, such as amines and organic sulfimides. When such a composition is required to cure under irradiation such as UV, it must also include at least one photoinitiator or sensitizer such as benzoin methyl ether or one of the initiators described in Australian Patent 469,564. The composition may also include polymeric thickeners, coloring agents including those pigments used in reflective coatings, and plasticizers. Free radical stabilizers may also be required to balance the shelf life' of the compositions against the speed of cure. These stabilizers are normally of the quinone type, and the preferred quinones are beta-naphthoquinone, 2-methoxy-l,4-naphthoquinone, and pbenzoquinone. Other stabilizers are disclosed in U. S. Patent 3,043,820. Compatible plasticizers may optionally be used, the preferred plasticizers being selected from the group of polyester polymeric plasticizers described in U. S. Patent 3,794,610. -3-.
The anaerobic character of these compositions has made them suitable for such applications as threadlocking, the retaining of bearings on shafts, and other bonding and/or sealing applications wherein oxygen is excluded from the joint. However, the anaerobic character of the compositions has also caused considerable problems. In the first place, the liquid remaining outside the threaded joint or the bond line remains in the liquid or tacky state and never fully cures. This can cause serious problems when small parts are packed together for shipment purposes, as the parts can eventually stick together and become unusable. When conventional anaerobic compositions are used to bond decorative articles, the tacky surface outside the joint easily collects dust from the atmosphere and produces an unsightly and often dirty line adjacent to the bonds. When the compositions are used in very fine machinery, such as watches, any excess composition outside the joint which does not cure can flow, into the working ihechanism and cause moving parts to seize.
An additional drawback has been the fact that, although the adhesives have excellent resistance to solvents and moisture and have good adhesion on a number of surfaces, they could never, because of their tacky outer surface, be used as coatings or potting materials for electronic parts.
Many methods are used today to reduce or abolish the inhibiting effect of atmospheric oxygen on the surface curing properties of acrylate-type compositions. It has been found 43764 that if irradiation-curable anaerobic curing compositlonw ore exposed to ultraviolet light in the presence of inert gases such as nitrogen with the exclusion of oxygen, then tack-free surfaces can be obtained. It has also been found that certain types of monomers are less sensitive to inhibition by oxygen than others and these have been used to produce improved compositions. Another method involves the inclusion in the composition of waxes which exude to the surface as polymerization proceeds and thereby form a barrier against inhibition of oxygen. However, this process is unsatisfactory since it leaves a waxy surface which often has to be removed by buffing or sanding before polishing. The wax in the material also reduces to some extent the adhesive properties of the cured compositions. Other methods involve the use of compatible compounds which are themselves reactive with oxygen in the presence of free radicals. In other cases the addition of chain transfer agents has been found to retard or eliminate the inhibiting effect of oxygen on polymerization. None of these methods has proven fully satisfactory, however.
SUMMARY OF THE INVENTION According to the present invention, there are provided anaerobic-curing compositions which, while stable in suitable oxygen-permeable containers, will nevertheless cure when unenclosed, even in the presence of oxygen. There is also provided a new method of excluding oxygen from unenclosed anaerobic-curing compositions so as to enable the compositions to cure. There is also provided a method of rendering nontacky anaerobic systems, as well as general purpose acrylate5 43764 based systems, the surface cure of which is inhibited by oxygen.
It has now been found that by including in the curable monomeric system a selected dry polymeric substance and a volatile solvent these compositions can be made to cure tackfree. On evaporation, the solvent deposits a thin film of the polymeric substance on the exposed surface of the liquid composition. This substantially excludes atmospheric oxygen from contact with anaerobic-curing material, which accordingly cures to a hard, tack-free solid. When one of these compositions of the invention is applied to the threads of a standard bolt and a mating nut is then assembled on the bolt, the anaerobic composition cures in the threads to effect a locking action. The excess anaerobic composition outside the threads also cures to a tack-free coating, which effect is both new and useful.
More specifically, the invention provides an anaerobically curable adhesive or coating composition comprising in admixture: an anaerobically curable portion comprising: (a) at least one acrylate or methacrylate monomer; (b) an initiator of free radical polymerization; and an additive portion comprising (c) an organic solvent compatible (as hereinafter defined) with the anaerobically curable portion which is not a monomer chosen for the anaerobically curable portion; (d) dissolved in the solvent 2 to 200 percent by weight vof the anaerobically curable portion of an organic polymer having an average molecular weight of more than ' l’ l· I - 6 42764 ,000 and a glass transition temperature of at least 0° C.; whereby, upon evaporation of at least some of the solvent, the exposed surface of the composition becomes nontacky and substantially resistant to the passage of oxygen, such that the corresponding anaerobic portion thereof is permitted to cure.
The invention also provides a method of rendering nontacky an anaerobically curable adhesive or coating composition containing at least one anaerobically curable acrylate or methacrylate monomer and a free radical initiator comprising (1) adding to such composition an organic solvent compatible (as hereinafter defined) with the anaerobically curable composition which solvent is not a monomer chosen for the anaerobically curable composition and in which solvent is dissolved 2 to 200 percent by weight of the anaerobically curable portion composition of an organic polymer having an average molecular weight of more than 10,000 and a glass transition temperature of at least 0°C, and (2) allowing at least a portion of the solvent to evaporate, thereby causing the exposed surface of the composition to become nontacky.
The invention also provides a method of excluding oxygen from an anaerobic curing composition.
As used herein, the term nontacky means that the exposed surface of the adhesive or sealant or coating composition is dry to the touch, not sticky, and does not adhere to contiguous exposed surfaces on similarly coated items in normal storage and handling.
Also as used herein, the term compatible means that the solvent must be miscible with the curable portion in the concentration used, must be readily, removable from the system by evaporation, and any solvent residue after evaporation must have no significant adverse effect on the cure of the curable portion. The invention provides an acrylate or methacrylate based curing composition which comprises, in addition to conventional ingredients, a film-forming quantity, in the sense . hereinbefore defined, of at least one organic polymeric substance. It is necessary that the polymeric substance have an average molecular weight of at least about 10,000. The molecular weight may be as high as 3,000,000, or even higher, provided that the polymeric substance remains soluble in a compatible solvent and has a sufficiently high glass transition temperature, as discussed below. Preferably, the molecular weight range will be from 10,000 to 1,000,000, more • preferably from 10,000 to 50,000. The polymeric substance should also have a glass transition temperature of at least 157 about 0°C, preferably from 20-120°C. It has been found that this combination of molecular weight and glass transition temperature is characteristic of organic polymers which are typically soluble in common organic solvents and exude to the surface of the curable composition upon evaporation of the solvent, thereby forming a nontacky, dry surface which is also resistant to the passage of oxygen. Suitable polymeric substances typically have an intrinsic viscosity of at least about 0.2. Preferably, the polymeric substance is selected from the class which comprises polyalkylmethacrylates, - polyacrylates, polyvinyl acetates, polyvinylidene chlorides, cellulose acetate butyrates and polyurethanes. The most preferred class of polymeric substances is the polyalkyl - 8 42764 methacrylates, such as polymethyl methacrylate and poly(isobutyl)methacrylate. Other polymeric substances may also be used, provided they meet the above-mentioned molecular weight and glass transition temperature requirements, can be dissolved in a compatible solvent, and are capable of producing a nontacky surface upon evaporation of at least some of the solvent.
The concentration of the polymeric substance must be related to its solubility in the chosen volatile solvent so that the substance quickly solidifies as a surface film of solid polymer after a relatively small quantity of the solvent has evaporated. Accordingly, the said concentration is in the range of 2% to 200% by weight of the anaerobically curable portion (i.e., monomer plus initiator and accelerator, if any) of the composition. Preferably, the concentration of the polymeric substance will be in the range of 3-160% by weight of the anaerobically curable portion of the composition. As a percentage of the total composition (i.e., curable portion plus additive portion), the concentration of the polymeric substance will usually be in the range of 1.5-60%, preferably 2-30%. Below 1.5%, there will ordinarily not be sufficient polymeric substance present to produce a tack-free surface of low oxygen permeability.
Above about 60%, the viscosity and other properties of the liquid concentration may be undesirably altered and properties of the cured composition may be degraded.
The solvent used must be compatible (as defined above) with the ingredients of the curable composition, and must not be 'a monomer chosen for the anaerobically curable composition. Chlorinated hydrocarbons are preferred. Ά second preferred class of 4(2764 solvents comprises reactive solvents, by which is meant that any solvent remaining in the composition after evaporation is able to copolymerize with the acrylate or methacrylate ingredients of the composition. Reactive solvents preferably are selected from the low molecular weight methacrylate esters, e.g., methyl methacrylate, butyl methacrylate, and isopropyl methacrylate. Compositions containing members of this class of solvents have the added advantage that voids and bubbles do not appear in the coating after aging. With nonreactive solvents (which continue to evaporate-during and even after cure), voids and cavities can occur which may be unsightly and which can give rise to a coating having lower resistance to chemicals and to the environment than when the preferred copolymerizing solvents mentioned above are used. The amount of solvent used will be a matter of routine experimentation, depending upon the solubility of the polymeric substance selected, the volatility of the solvent, the desired viscosity of the composition, and such other considerations as would-be apparent to those skilled in the art. In general, the solvent concentration is not critical and may range from 2t98% by weight of the total composition.
’ As had been indicated, the compositions of this invention are rendered nontacky while still in their uncured (or perhaps slightly cured) condition by evaporation of at least - 10 43764 some portion of the solvent. Ideally, the solvent is entirely evaporated; however, this is not a necessity in all cases.
The key requirement is that sufficient solvent be removed to cause deposition at the surface of the anaerobically curable ccnposition of sufficient polyneric substance to cause the anaerobically curable composition to be nontacky. Thus, the exact amount of solvent which must be removed in any given composition is a matter of simple experimentation and will, of course, depend upon the particular ingredients used. The necessary evaporation may be allowed to occur naturally by the volatile nature of the solvent, or the rate of evaporation may be quickened by application of heat or vacuum. If all the solvent is not to be removed, obviously it must be sufficiently removed that the residue does not significantly interfere with the cure or properties of the composition. Of course, in the case of reactive solvents, it may be permissible, and even desirable, to leave a substantial quantity of the solvent behind for coreaction with the monomer or monomers.
The monomer used can be any of a wide variety of known, free radical curable acrylate and alkyl acrylate (e.g., methacrylate) types. Typical of such materials would be methylmethacrylate. Anaerobically curable canpositions based on such ironaners are polymerized through the action of known free radical generating initiators, such as benzoyl peroxide, methylethyl ketone peroxide, azobisisobutyronitrile, among others. Such initiators are activated by application of moderate heat, as is well known in the art. - 11 42764 Numerous ul'traviolet-sensitive free radical generators are also well known for such monomer systems.
The preferred monomers for use in the present compositions are those normally associated with anaerobic curing properties, as previously mentioned. One particularly useful class of monomers is that described in U. S. Patent 3,425,988, mentioned above. These monomeric polyacrylate esters may be made in a variety of ways; however, the method which has proven most eminently suited involves the reaction of a mono10 functionally substituted alkyl or aryl acrylate ester containing an active hydrogen atom on the functional substituent. This monofunctional, acrylate-terminated material is reacted with an organic polyisocyanate in suitable proportion so as to convert all of the isocyanate groups to urethane or ureido groups. The monofunctional alkyl and aryl acrylate esters are preferably the acrylates and methacrylates containing hydroxy and amino functional groups on the nonacrylate portion thereof. Acrylate esters suitable for use in this invention have the formula R^O H2C=C-C-O-R5-X-H (1) · wherein X is selected from -o- and.
R ι -Bland wherein R is a hydrogen atom or an alkyl group of 1 to 7 carbon atoms; R1 is a hydrogen or a chlorine atom or a methyl ( - 12 42764 R^O 0 h2c=c-c-o-r2-X-C-NH2 ethyl radicalρ and R is a divalent organic radical which is an alkylene radical with 1 to 8 carbon atoms, a phenylene or a naphthylene radical. These groups, upon proper reaction with a polyisocyanate, yield a sealant monomer of the following formula: —B (2) n 2 wherein R , R and X are as defined above; n is an integer from 2 to 6 inclusive; and B is an n-valent organic radical derived from an alkyl, alkenyl, cycloalkyl, aryl, aralkyl, alkaryl or heterocyclic radical either substituted or unsubstituted.
As used herein the terms acrylate and polyacrylate include the methyl, ethyl and halogen homologues thereof.
The hydroxy- and amine-containing materials suitable for use in the preparation of the above monomeric products are exemplified by but not limited to such materials as hydroxy ethyl acrylate, hydroxy ethyl methacrylate, amino ethyl methacrylate, 3-hydroxy propyl methacrylate, amino propyl methacrylate, hydroxy hexyl acrylate, t-butylaminoethyl methacrylate, and hydroxy octyl methacrylate.Illustrative of the polyisocyanates employed are, among others, toluene diisocyanate, 4,4'-diphenyl diisocyanate, 4,4*-diphenylene methane diisocyanate, dianisidine diisocyanate, 1,5-naphthalene diisocyanate, 4,41-diphenyl ether diisocyanate, p-phenylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, ethylene diisocyanate, cyclohexylene diisocyanate, nonamethy13 lene diisoeyanate, octadecamethylene diisoeyanate, 2-chloropropane diisoeyanate, 2,2'-diethylether diisoeyanate, 3(dimethylamine)pentane diisoeyanate, tetrachlorophenylene diisoeyanate, 1,4-3-heptene diisoeyanate and transvinylene diisoeyanate. Still other polyisocyanates that may be used are the higher molecular weight polyisocyanates obtained by reacting polyamines containing terminal, primary and secondary amine groups or polyhydric alcohols, for example, the alkane and alkene polyols such as glycerol, 1,2,6-hexanethanol, 1,510 pentanediol, ethylene glycol, polyethylene glycol, bisphenol-A, 4,4'-dihydroxyphe'nyldimethylmethane substituted bisphenol-A, with an excess of any of the above-described isocyanates.
These higher molecular weight urethane or ureide polyisocyanates may be represented by the formula: H 0 O=C=N-R3-N-C-X--B n (3) wherein Β, X and n have the meanings set forth above and R3 is an alkylene, alkeny-lene, cycloalkylene, arylene, aralkylene or alkarylene radical of 2 to 20 oarbon atoms.
Preferred organic polyisocyanates comprise the higher 20 alkenyl diisooyanates, the cycloalkenyl diisocyanates and the aromatic diisooyanates containing more than 8 carbon atoms and ' preferably from 15 to 30 carbon atoms, such as, for example, · ‘octamethylene diisoeyanate, durene diisoeyanate, 4,41-diphenyl diisoeyanate, and the higher molecular weight polyisocyanate 25 reaction products mentioned hereinbefore. 43764 Further detail may bo obtained by reference to U. S. Patent 3,425,988.
Other useful monomers are the polyacrylate esters represented by the formula Γ 4 Ί 4 R 0 0 R ... ' H.C=C-C-0--[M-Ol-C-C =CH_ (4) 2 p 2 wherein R is a hydrogen or a halogen atom or an alkyl group of from 1 to 4 carbon atoms; p is an integer equal to at least 1, and preferably equal to from 1 to 4; and M is an organic radical containing at least two carbon atoms and having a total bonding capacity of p plus 1. With regard to the upper limit for the number of carbon atoms in M, workable monomers exist at essentially any value. As a practical matter, however, a general· upper limit is about 50 carbon atoms, preferably 30, and most preferably 20·.· For example, M can be an organic radical of the formula 0 i 9 -Y -OCZC-OY 2 wherein each of Y and Y is an organic radical, preferably a hydrocarbon group, containing at least 2 carbon atoms, and preferably from 2 to 10 carbon atoms, and Z is an organic radical, preferably a hydrocarbon group, containing at least 1 carbon atom, and preferably from 2 to 10 carbon atoms.
Other classes of useful polyacrylate ester monomers are the reaction products of di- or tri-alkylolamines (e.g., - 15 43764 ethanolamines or propanolamines) with acrylic acids, such as are disclosed in .French Patent No. 1,581,361.
Still other useful monomers are polyacrylate esters which have the following formula: wherein R3 represents a hydrogen atom, a lower alkyl radical of from 1 to 4 carbon atoms, a hydroxy alkyl radical of from 1 to 4 carbon atoms, or a radical of the formula 9 -CH»-O-C-C=CH2 i*2 R4 where R4 is as defined above; R6 is a hydrogen atom, a hydroxyl group or a radical of the formula 0 B2 -O-C-X=CH q is an integer equal to at least 1, e.g., from I to 15 or higher, and preferably from 1 to 8 inclusive; s is an integer equal to at least 1, e.g., 1 to 40 or more, and preferably from 2 to 10; and r is 0 or 1.
Typical examples of polyacrylate esters corresponding to the above formula are di-, tri- and tetraethyleneglycol dimethacrylate, di(pentamethyleneglycol) dimethacrylate, tetraethyleneglycol diacrylate, tetraethyleneglycol di (chloroacrylate), diglycerol diacrylate, diglycerol tetramethacrylate, butyleneglycol dimethacrylate, neopentylglycol - 16 42764 diacrylate, and trimethylolpropane triacrylate.
While di- and other polyacrylate esters ( and particularly the polyacrylate esters described in the preceding paragraphs ) have been found particularly desirable, mono5 acrylate esters also may be used. When dealing with monoacrylate esters, it is highly preferable to use an ester which has a relatively polar alcoholic moiety. Such materials are less volatile than low molecular weight alkyl esters and, more important, the polar group tends to provide intermolecular attraction during and after cure, thus producing more desirable cure properties, as well as a more durable sealant or adhesive. Most preferably the polar group is selected from labile hydrogen, heterocyclic ring, hydroxy, amino, cyano, and halogen polar groups. Typical examples of compounds within this category are cyclohexylmethacrylate, tetrahydrofurfury.l methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, t-butylaminoethyl methacrylate, cyanoethylacrylate, and chloroethyl methacrylate. Anaerobic compositions based on such monoacrylates are de20 scribed more fully in U. S. Patent 3,435,012·.
Still another useful class of monomers is that disclosed by U. S. Patent 3,944,521. These monomers have the formula ,7 R· .9 R' 0-R (6) 42784 wherein the aromatic groups are substituted or unsubstituted g 7 n benzene rings or other aromatic groups; R and R are hydrogen, alkyl, aryl, hydroxyalkyl groups, or halogen; and R? and r8 are 5 CH_=C—C(0—CH—CH) I II I V X RU0 R12 R13 wherein x is an integer from 1 to 20 and preferably 1 to 5, 12 13 and R , R and R are hydrogen, alkyl, alkoxy groups, or halogen.
Examples of aromatic groups other than benzene are naph10 thalene, anthracene and other polynuclear groups. The alkyl groups may be methyl, ethyl and other primary, secondary or tertiary alkyl groups and the hydroxyalkyl groups, for example, hydroxyethyl. The preferred halogen is chlorine.
A preferred monomer of this class is the dimethacrylate of propoxylated bisphenol-A, the number of propoxyl residues in the chain being preferably 1 to 5; others are propoxylated bisphenol-C dimethacrylate, ethoxylated bisphenol-A dimethacrylate, and ethoxylated bisphenol-A diacrylate.
As indicated above, the anaerobic compositions as discussed herein are prepared by mixing a peroxy initiator with one or more acrylate esters as described above. While certain peroxides (generally dialkyl peroxides) have been disclosed as useful initiators in, e.g., U. S. Patents 3,419,512 and 3,479,246, the hydroperoxides are far ' superior and constitute a highly preferred embodiment.
The real benefit of the nonhydroperoxide initiators is as co-initiators with the hydroperoxides to make the cure proper ties of the anaerobic composition more universal.
Hydrogenperoxide may be used, but the most desirable polymerization initiators are the organic hydroperoxides. Included within this definition are materials such as organic peroxides or organic peresters which decompose or hydrolyze to form organic hydroperoxides in situ. Examples of such peroxides and peresters are cyclohexyl and hydroxycyclohexyl peroxide and t-butyl perbenzoate, respectively.
While the nature of the organic hydroperoxides is not critical to the broad concept of this invention, the general class of hydroperoxides can be represented by the formula 14 14 R OOH, wherein R generally is a hydrocarbon group containing up to .18 carbon atoms, and preferably is an alkyl, aryl or aralkyl hydrocarbon group containing from 14 to 12 carbon atoms. Naturally R can contain any substituent or linkage, hydrocarbon. or otherwise, which does not affect the hydroperoxide adversely for the purpose disclosed herein. Typical examples of such organic hydroperoxides are cumene hydroperoxide, tertiary butyl hydroperoxide, methylethylketone hydroperoxide, and hydroperoxides formed by oxygenation of various hydrocarbons such as methylbutene, cetane, and cyclohexene, and various ketones and ethers, including certain compounds represented by formula 5, above.
The organic hydroperoxide initiators can be used within wide ranges, e.g., up to 20% by weight of the composition. Most commonly, however, they comprise no more than 10.percent by weight of the composition since above that level adverse effects on the strength and durability of the cured composition may be experienced. While in some instances lower amounts can be used, o.l% by weight of the compo- 19 4376 4 sition is a common--lower limit. Preferably the hydroperoxide initiator comprises from 0.1% to 5% by weight of the composition.
Common additives for anaerobic compositions are latent polymerization accelerators, compounds which do not of themselves initiatecure, but which accelerate the cure once it has been started Ly th,e polymerization initiator. It should be noted that large numbers of polymerization accelerators are known in the art, and the broad concept of this invention is intended to encompass any polymerization accelerator which can be incorporated in the anaerobic composition without destroying the essential characteristics of such composition.
Among the earliest of the polymerization accelerators used in anaerobic compositions were amines. The most commonly used are tertiary amines such as tributylamine and triethylamine. Essentially the entire class pf tertiary amines can be used in such compositions, and the class may be broadly represented by the formula NR15R16R17 wherein each of R^, r16 and R^7 is a hydrocarbon group containing up to ten carbon atoms. Naturally, the hydrocarbon groups can contain any substituent or linkage which does not adversely affect the ability of the amine to perform its intended function. Preferably, each of R^, r·*·6 and R^7 is an alkyl, aryl or aralkyl group containing up to 8 carbon atoms. - 20 42764 The Ν,Ν-dialkyl aryl amines are particularly effective tertiary amines. Typical amines within this class may be represented by the following general formula: R18 l-E— (R20)t wherein E represents a carbocyclic aromatic nucleus which is a phenyl or naphthyl radical; R18 and R19 are hydrocarbon groups containing up to 10 carbon atoms; and preferably are lower alkyl radicals of 1 to 4 carbon atoms, t is O or an integer from 1 to 5 inclusive; R20 is a hydrocarbon group containing up to 5 carbon atoms, ’and preferably is an alkyl or alkoxy radical of 1 to 4 carbon atoms Inclusive, provided that when an R20 radical is in the ortho position t is greater than 1.
Primary and secondary amines also can be used as accelerators in the anaerobic compositions of this invention. Particularly good primary and secondary amines are the primary and secondary alkyl amines, most particularly those wherein each alkyl group contains up to 10 carbon atoms. A separate and highly preferred class of secondary amines has been found to be the class of heterocyclic secondary amines, particularly heterocyclic secondary amines containing up to 20 carbon atoms. it also is preferred to use those amines wherein the heterocyclic ring is hydrogenated. Typical of such compounds are pyrrolidine, piperazine and 1,2,3,4tetrahydroquinoline. α ά 7:β a Another highly successful class of accelerators is the organic sulfimides, i.e., organic compounds which contain the 9rouP OHO η ι ti -S-N-CI Because of the extreme effectiveness of the sulfimides as accelerators fox anaerobic compositions, compositions containing sulfimides constitute a highly preferred embodiment of the invention disclosed herein. While the broad class of organic sulfimides can be used successfully, the sulfimides most commonly used can be represented by the formula OHO ti ι ti 99 R -S-N-C-RZZ . 21 22 wherein each tjf R. and R is a hydrocarbon group containing up to ten carbon atoms, and preferably up to six 21 22 carbon atoms. Naturally R and R can contain any linkage or substituent which does not adversely affect the sulfimide for its intended use in the anaerobic composition. Further, 22 R and R can be united to bond the sulfimide group m a heterocyclic ring, or a polynuclear heterocyclic ring system. Of the organic sulfimides, benzoic sulfimide has been found to be the most preferable.
An even more highly preferred composition is that which contains a sulfimide, particularly benzoic sulfimide, in combination with either a heterocyclic secondary amine or a tertiary Ν,Ν-dialkyl aryl amine, both of which are described above. For an expanded discussion of this type of system, reference is made to U. S. Patent 3,218,305.
Other less active accelerators can be used in the compositions of this invention. Typical examples of such accelerators are succinimide, phthalamide and formamide.
Routine testing will easily determine the optimum amount of accelerator which can be incorporated in a given anaerobic composition. However, the following general guidelines may be used. With regard to tertiary amines, large amounts may be used if desired, up to '8 percent by weight of the composition, or higher. However, little if any additional benefit is obtained above about 5 percent. Most preferably these tertiary amine accelerators are used at from 1 percent to 4 percent by weight of the anaerobic composition.
The succinimide, phthalamide and formamide accelerators also can be used in significant amounts, up to 8 percent by weight of the composition, or higher, and preferably from Γ percent to 5 percent by weight. The sulfimide and heterocyclic secondary amine accelerators generally are used at less than 4 percent by weight of the anaerobic composition. In the special case where a sulfimide is used in combination with a heterocyclic secondary amine or an N,Ndialkyl arylamine, the total of the two accelerators preferably does not exceed 4 percent by weight of the anaerobic composition, and either component does not exceed 3 percent by weight.
Other ingredients can be used in the anaerobic compositions useful to this invention, and in its preferred aspects polymerization inhibitors are included to offer protection against spurious polymerization prior to the time of intended !! 43Ϊ64 use. The quinones have been found to be a particularly effective class of polymerization inhibitors, and can be used herein. Examples of such quinones are beta-naphthoquinone, 2methoxy-1,4-naphthoquinone, and p-benzoquinone. Compositions containing such inhibitors are described more fully in U. S. Patent 3,043,820, mentioned above.
Other typical functional ingredients which can be used if desired to impart commercially desirable properties to the composition are thickeners, dyes, adhesive agents, thixo10 tropic agents, and plasticizers, especially those polyester plasticizers described in 0. S. Patent 3,794,610.
Such functional materials can be used in such combination and proportions as desired, provided they do not adversely affect the nature and essential properties of the composition.
While exceptions may exist in some cases, these materials in toto generally do not comprise more than . 50% by weight of the total composition, and preferably not more than 20% by weight of the composition. The above-described anaerobic compositions generally can be prepared by the use of any conventional mixing techniques. Certain other ingredients which may desirably be added may not possess ready solubility, and if such additives are used (e.g., silica), it may be desirable to use high-shear mixing.
The following examples illustrate, but do not limit, the invention. - 24 48764 Example 1 This example shows comparative data for normal anaerobic curing compositions compared with compositions of the invention.
Monomer I used in this Example has the formula (ch3) coocHga^ooa® -(PR) in which (PR) represents the propylene triol oligomer devoid of its three hydroxyl groups. A general process for preparing Monomer I, among others, is given in Patent Specification No. 39134.
Compositions A, B and C were made up by simple admixture of the following ingredients in the proportions given: 1. Monomer I 2. Ethoxylated bisphenol-A diacrylate 3. Benzoin isobutyi ether 4. Cumene hydroperoxide . Poly(methylmethacrylate) 6. Methylmethacrylate Total weight prepared Parts by Weight A_B_C --95 4 4 111 77-140g lOg 50g Ingredient 5 is the polymeric substance used in the invention. It has an intrinsic viscosity in chloroform at °C between 2.5 and 3.0 and is supplied by Imperial Chemical 2764 Industries, Limited under the product reference CA-603.
Ingredient 6 is the volatile solvent; it is a reactive solvent in the sense described above. Ingredient 3 is a photoinitiator which reacts to DV-irradiation by releasing free radicals.
Ingredient 4 is a peroxy catalyst, which forms free radicals. Ingredients 1 and 2 are polymerisable monomers in the sense current in the art, which can polymerise to form the anaerobicall cured adhesive or coating composition.
It will be seen that compositions B and C are conventional, each requiring the addition of a portion of composition A to convert it into a Composition of the invention.
Compositions A (90g) and B (lOg) were thoroughly mixed to yield composition D of the invention. Composition A (50g) and C (50g) were thoroughly mixed to yield composition E of the invention.
Each of composition B and C (of the prior art) and D and E (of the invention) was tested as follows. A thin film of the composition was spread over a microscope slide and exposed to a Philips MB/U (Phillips'is a ; : ·’ Trade Mark) 40020 watt ultraviolet lamp at a distance of 10cm.
All the compositions were converted to hard solids B. and D in 2 minutes, C and E in 1 minute.
The prior art compositions B and C retained greasy or tacky surfaces, which remained thus even after several hours, whereas the compositions D and E of the invention became dry to the touch within 30 seconds of exposure tp the lamp, and remained dry indefinitely thereafter.. .26 4 376 4 Example 2 Compositions F and G were made up by simple admixture of the following ingredients in the proportions given: Parts by Weight 5 F G Ethoxylated bisphenol-A diacrylate 95 - Cumene Hydroperoxide 4.5 3.5 Tributyl amine 0.5 0.5 Poly(methylmethacrylate) - 19 10 Methylmethacrylate - 77 Total Weight prepared 25g 75g Composition F was thoroughly mixed with composition G to make composition H.
Bonds were made by applying adhesive to a grit blasted 15 flat surface of mild steel. Another surface of steel was placed over the first and the two clamped together with a spring clamp. This was done using composition H and also composition F.
After 5 hours the clamps were removed and the metal parts 20 were found to be strongly bonded together. The excess adhesive outside the bond made with composition F was wet to the touch. The excess adhesive outside the bond made with composition H was dry to the touch.
Example 3 Compositions J and K were made up as shown below: Parts by Weight J K Poly(methyl,n-butylmethacrylate) (Elvaeite·2013 - DuPont) (the word 31 Elvaeite being a Trade Mark) Ethylene glycol\dimethacrylate 69 - Monomer II 45.0 Monomer I 20.6 Hydroxypropylmethacrylate 28.6 Acrylic Acid 2,8 Tributyl amine 0.3 Cumene hydroperoxide 2.6 Monomer X is as defined above. Monomer ΙΪ has the formula CH2=C(CH3)COOC^HgOCONH HOCO-θ-, (CH,) 3'2 A general process for preparing Monomer IX is given in Patent Specification No» 39134 above cited.
To 90 parts by weight of formulation K were added 10 parts of J to form, after mixing, formulation L. !0 Thin films of formulations K and L were spread over glass surfaces (microscope slides) and heated in an oven at 105°C for twenty minutes. They then were cooled to a temperature of . 35°C. At that temperature the surface of formulation K was tacky, that of formulation L was not.

Claims (12)

1. CIAIMS:1. An anaerobically curable adhesive or coating composition comprising in admixture: an anaerobically curable portion comprising 5 (a) at least one acrylate or methacrylate monomer; (b) an initiator of free radical polymerisation; and an additive portion comprising (c) an organic solvent compatible (as hereinbefore defined) with the anaerobically curable portion which is not a monomer 10 chosen for the anaerobically curable portion; (d) dissolved in the solvent
2. To 200% by weight of the anaerobically curable portion of an organic polymer having an average molecular weight of more than 10,000 and a glass transition temperature of at least 0°C; 15 whereby upon evaporation of at least some of the solvent the exposed surface of the composition becomes nontacky and substantially resistant to the passage of oxygen, such that the corresponding anaerobic portion thereof is permitted to cure. 20 2. A composition as claimed in claim 1 wherein the initiator is a UV initiator.
3. A composition as claimed in claim 1 wherein the initiator is an organic peroxide.
4. A composition as claimed in any of claims 1 to 3 25 wherein the solvent is a chlorinated hydrocarbon. ' 5. A composition as claimed in any of claims 1 to 3 wherein the solvent is a reactive solvent (as hereinbefore defined). 6. A composition as claimed in any of claims 1 to 5 wherein the organic polymer is a polyacrylate or a polyalky lmethacry late .
5. 7. An anaerobically curable adhesive or coating composition comprising in admixture; an anaerobically curable portion comprising (a) at least one acrylate or methacrylate monomer; (b) an organic hydroperoxide or perester initiator of free 10 radical polymerisation; and an additive portion comprising (c) an organic solvent compatible (as hereinbefore defined) with the anaerobically curable portion, Which is not a monomer chosen for the anaerobically curable portion; (d) dissolved in the solvent 2 to 200% by weight of the 15 anaerobically curable portion of an organic polymer having an average molecular weight of more than 10,000 and a glass transition temperature of at least 0°C; whereby upon evaporation of at least some of the solvent the exposed surface of the composition becomes nontacky 20 and substantially resistant to the passage of oxygen, such that the corresponding anaerobic portion thereof is permitted to cure.
6. 8. A composition as claimed in claim 7 wherein the initiator is cumene hydroperoxide. 25
7. 9. A composition as claimed in claim 7 or 8 which contains in addition a UV initiator. - 30
8. 10. A composition as claimed in any of claims 7 to 9 wherein the solvent is a chlorinated hydrocarbon.
9. 11. A composition as claimed in any of claims 7 to 9 wherein the solvent is a reactive solvent (as hereinbefore defined).
10. 12. A composition as claimed in any of claims 7 to 11 wherein the organic polymer is a polyacrylate or a polyalky Imethacry late .
11. 13. An anaerobically curable adhesive or coating composition including an organic polymer having an average molecular weight of more than 10,000 and a glass transition temperature of at least 0°C substantially as described with particular reference to any of the Examples excluding the comparative material.
12. 14. A method of rendering nontacky an anaerobically curable adhesive or coating composition containing at least one anaerobically curable acrylate or methacrylate monomer and a free radical initiator comprising (1) adding to such composition an organic solvent compatible (as hereinbefore defined) with the anaerobically curable composition which solvent is not a monomer chosen for the anaerobically curable composition and in which solvent is dissolved 2 to 200% by weight of the composition of an organic polymer having an average molecular weight of more than 10,000 and a glass transition temperature of at least 0°C and (2) allowing at least a portion of the solvent t0 evaporate, thereby causing the exposed surface of the composition to become nontacky. F. R. KELLY & CO.,
IE282575A 1975-12-30 1975-12-30 Nontacky coating and adhesive compositions IE42764B1 (en)