FI124954B - Menetelmä kultaa sisältävän liuoksen valmistamiseksi ja prosessijärjestely kullan ja hopean talteenottamiseksi - Google Patents

Menetelmä kultaa sisältävän liuoksen valmistamiseksi ja prosessijärjestely kullan ja hopean talteenottamiseksi Download PDF

Info

Publication number
FI124954B
FI124954B FI20135448A FI20135448A FI124954B FI 124954 B FI124954 B FI 124954B FI 20135448 A FI20135448 A FI 20135448A FI 20135448 A FI20135448 A FI 20135448A FI 124954 B FI124954 B FI 124954B
Authority
FI
Finland
Prior art keywords
gold
solution
silver
leaching
extraction
Prior art date
Application number
FI20135448A
Other languages
English (en)
Swedish (sv)
Other versions
FI20135448A (fi
Inventor
Ville Miettinen
Riina Ahtiainen
Kari Valkama
Erkki Paatero
Kari Hietala
Mika Haapalainen
Original Assignee
Outotec Oyj
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Priority to FI20135448A priority Critical patent/FI124954B/fi
Application filed by Outotec Oyj filed Critical Outotec Oyj
Priority to PE2015002302A priority patent/PE20151792A1/es
Priority to EA201591948A priority patent/EA029330B1/ru
Priority to CA2910033A priority patent/CA2910033C/en
Priority to CN201480028817.8A priority patent/CN105378121A/zh
Priority to PCT/FI2014/050309 priority patent/WO2014177765A1/en
Priority to BR112015027156A priority patent/BR112015027156B8/pt
Priority to MX2015014993A priority patent/MX367751B/es
Priority to US14/787,404 priority patent/US10060007B2/en
Priority to EP14791228.1A priority patent/EP2992119B1/en
Priority to AU2014261257A priority patent/AU2014261257B2/en
Publication of FI20135448A publication Critical patent/FI20135448A/fi
Application granted granted Critical
Publication of FI124954B publication Critical patent/FI124954B/fi
Priority to PH12015502440A priority patent/PH12015502440A1/en
Priority to CL2015003158A priority patent/CL2015003158A1/es
Priority to ZA2015/08041A priority patent/ZA201508041B/en

Description

Method of preparing a gold-containing solution and process arrangement for recovering gold and silver
Field of the invention
The present invention relates to a method for preparing a gold-containing solution by chloride leaching from gold-bearing raw materials. A further object of the invention is to provide a method for recovering gold and optionally silver from the prepared gold-containing solution. The invention relates also to a process arrangement for recovering gold and silver.
Background of the invention
Nowadays cyanide leaching is considered as the best option for leaching gold from gold-containing ores and concentrates. Another option is chloride leaching, but even though the use of chloride for gold leaching has been known for a long time, it has not been extensively applied in commercial practice. Chloride leaching has been considered too expensive due to relatively high reagent (oxidant) consumptions. The recovery of gold from chloride leach solutions has also been considered challenging, and the recovery yield has been lower than in cyanide leaching. Furthermore, there are corrosion problems because of high chloride concentrations of the leaching solutions. US 4 551 213 discloses a method of recovering gold values from sulphur-containing ore mixtures by leaching with chlorides (alkali metal chloride and/or alkali earth metal chloride), oxidizing agent (chloride gas) and cupric or ferric chloride. It is recited that the concentration of chloride in the leaching may be 12 to 47 weight-% and the concentration of cupric or ferric chloride 3.5 to 27 weight-%. A leaching temperature of about 20 to 106°C, preferably about 40 to 80°C, is disclosed. In the examples, the leaching is performed at a temperature of 60 to 65°C. The sulphur-containing ore used as the starting material may be obtained from hydrometallurgical processing of copper, for example. Gold may be recovered from the leach solution electrolytically or by adsorption on carbon. EP 1 583 848 B1 discloses a process for recovering precious metals, such as gold, from sulfidic materials, by leaching with a mixture containing a mixture of halides and multivalent metal compounds selected from copper, iron, cobalt, manganese and vanadium compounds. Typical starting materials for the process are refractory gold concentrates, such as arsenopyrite (optionally with pyrite and/or with carbon). The mixture of halides in the leaching pref erably comprises chloride and bromide. The multivalent metal in the metal halide leaching solution is typically copper (Cu2+). The leaching may be performed at a temperature of 90 - 105°C. Leaching pH values in the range of less than 1 but greater 0.2 are disclosed. The precious metal may be recovered from the leach solution by adsorption on carbon (activated carbon), or by ion exchange, solvent extraction, etc. From the recovery stage, the solution is typically recycled to the leaching stage.
According to Examples 1 - 3 of EP 1 583 848 B1, gold was recovered from a single refractory Au concentrate by a two-step or one-step leaching process at a temperature of 105°C with a leach solution comprising NaCI, CaCb, Cu (from CuCb) and HCI. CA 2 599 174 discloses a method of leaching gold from copper sulphide ores, where the sulphide ore is first subjected to leaching of copper, followed by leaching gold from the leach residue with a leach liquor containing chloride ions and ferric and ferrous ions. It is also recited that the rate of gold leaching reaction can be enhanced by the co-presence of either copper or bromide ion or both together in the leach liquor. A leaching temperature of 80°C or more is disclosed. According to Example 6, copper is first leached from a copper sulphide concentrate, whereafter gold was extracted from the leach residue with a leach liquor containing Cu, Cl and Br at a temperature of 85°C.
Further processes for gold recovery have been disclosed in the textbook "The Chemistry of Gold Extraction", J. Marsden and lain House, Society for Mining, Metallurgy and Exploration Inc., 2006, p. 275. These processes include a commercial leaching process of a silver-bearing material at 75°C with a near-saturated solution of sodium chloride with hydrochloric acid (pH 0.3) and 15 g/l ferric ion as the oxidant. A further process comprises an atmospheric leaching process using NaCI and NaOCI at pH 7 from gold ores containing cyanide-soluble copper. A still further process consists of high temperature (200 to 225°C) pressure oxidation in sulphate media containing 5 to 20 g/l NaCI, particularly proposed for gold-bearing starting materials containing byproducts such as copper, nickel, and platinum group metals. WO 2011/154603 A1 (15.12.2011) discloses a method of recovering gold by solvent extraction from an acidic chloride-containing aqueous solution or from a slurry containing gold-bearing solids. The solvent extraction is performed with a diester of 2,2,4-trialkyl-1,3-pentanediol. The gold-bearing organic solution obtained from the extraction is scrubbed with an acidic aqueous solution, after which gold is stripped into water, from where it is reduced to form pure gold.
Brief description of the invention
An object of the present invention is to provide an improved method for preparing a gold-containing solution by chloride leaching from gold-bearing raw materials. A further object of the invention is to provide a method for recovering gold from the prepared gold-containing solution by solvent extraction. The objects of the invention are achieved by a method and a process arrangement, which are characterized by what is stated in the independent claims. The preferred embodiments of the invention are disclosed in the dependent claims. A further object of the invention is to provide a process arrangement for recovering gold and silver.
The invention is based on selecting a suitable chloride-based leaching solution and suitable leaching conditions for dissolving gold from gold-bearing raw materials with good yield. The method of the invention may be combined with efficient circulation of the chloride-based leaching solution. Gold can then be conveniently recovered from the gold-containing leach solution by different methods, such as solvent extraction.
The method of the invention provides an economical and efficient way of recovering gold by chloride-based leaching from gold-bearing raw materials, such as gold ores and concentrates, contrary to the current prejudices in the field against the application of chloride-based processes for gold leaching. Besides gold, silver can be conveniently recovered in the same process.
Brief description of the drawings
In the following the invention will be described in greater detail by means of preferred embodiments with reference to the attached drawings, in which
Figure 1 is a block diagram of an exemplary embodiment of the invention, showing also silver recovery;
Figure 2 depicts the effect of the copper concentration on the gold concentration in the leach solution of test 3 of Example 1 i.e. Gold concentration of the solution vs. copper concentration in test 3 of Example 1: [Cu]aq=50-100 g/l, [NaBr]aq,o=100 g/l, [CaCl2]aq,o=177 g/l, acid concentration >10 g/l (HCI), T-98°C, oxygen feed 500-2000 ml/min, and solid concentration 200 g/l;
Figure 3 depicts the effect of the bromide concentration on the gold concentration in the leach solution of test 4 of Example 1 i.e. Gold concentration of the solution vs. bromide concentration in test 4 of Example 1: [Cu]aq,o=100 g/l, [NaBr]aq=10-100 g/l, [CaCI2]aq,o=177 g/l, acid concentration >10 g/l (HCI), T=98°C, oxygen feed 220 ml/min, and solid concentration 200 g/l;
Figure 4 depicts the effect of the leaching time on the gold concentration in the leach solution of test 1 of Example 2; i.e. Gold concentration of the solution vs. leaching time in test 1 of Example 2: [Cu]aq,o=100 g/l, [NaBr]aq=10-100 g/l, [CaCI2]aq,o=177 g/l, pH=1.7, T=98°C, oxygen feed 2 l/min, and solid concentration 200 g/l;
Figure 5 depicts the effect of the copper concentration on the gold concentration in the leach solution of test 3 of Example 2; Gold concentration of the solution vs. copper concentration in test 3 of Example 2: [Cu]aq,o=0-75 g/l, [NaBr]aq=100 g/l, [CaCI2]aq,0=177 g/l, pH=1.7, T=98°C, oxygen feed 2 l/min, and solid concentration 400 g/l;
Figure 6 depicts the effect of the bromide concentration on the gold concentration in the leach solution of test 4 of Example 2 i.e. Gold concentration of the solution vs. bromide concentration in test 4 of Example 2: [Cu]aq,o=100 g/l, [NaBr]aq=0-60 g/l, [CaCI2]aq,o=177 g/l, pH=1.7, T= 98°C, oxygen feed 2 l/min, and solid concentration 400 g/l.;
Figure 7 depicts the effect of the chloride concentration on the gold concentration in the leach solution of test 5 of Example 2 i.e. Gold concentration of the solution vs. chloride concentration in test 5 of Example 2;
Figure 8 depicts the gold concentration in the leach solution vs. leaching time in the comparative cyanide test of Example 3 i.e. Gold concentration of the solution in cyanide test in Example 3: [NaCN]aq=3 g/l, pH=11, T=25°C, solid concentration 33 w-%, and air feed 0.5 ml/min;
Figure 9 depicts the effect of the leaching time on the gold concentration in the leach solution of tests 1 and 2 of Example 3 i.e. Gold concentrations vs. leaching time in tests 1 and 2 of Example 3. Test 1: [Cu2+]aq,o=100 g/l, [NaBr]aq,o=100 g/l, [Cr]aq,o=225 g/l, [solid]0=50 g/l, pH=1.7, T= 98°C, oxygen feed 1.5 l/min, and material from POX test 1. Test 2: [Cu2+]aq!o=20 g/l, [NaBr]aq,o=8-100 g/l, [CI']aq,o=150 g/l, [solid]0=315 g/l, [acid]Hci=10 g/l, T-98°C, oxygen feed 2 l/min, and material from POX test 1;
Figure 10 is an example embodiment of the process arrangement.
Detailed description of the invention
The invention relates to a method of preparing a gold-containing solution from gold-bearing raw material. The method of the invention comprises (a) a gold leaching step, wherein the gold-bearing raw material is subjected to oxidative chloride leaching in an aqueous leaching liquor in the following conditions: (i) the aqueous leaching liquor contains dissolved cupric ions (Cu2+), chloride (Cl') and bromide (Br"), (ii) pH is within a range wherein the cupric ion does not precipitate, (iii) the oxidation potential is at least 450 mV Pt vs. Ag/AgCI, to provide a gold-containing solution.
The gold-containing solution may optionally further contain silver. The method may further comprise a liquid/solid separation step (b), wherein the gold-containing solution is separated from the undissolved solid material; a gold recovery step (c), wherein gold is recovered from the gold-containing solution from step (b) to obtain a gold-bearing organic solution and a gold-depleted leach solution containing Cu2+, Cl' and Br', and optionally a circulation step (d), wherein the gold-depleted leach solution containing Cu2+, Cl' and Br' is circulated to the leaching step (a).
Starting materials
The gold-bearing raw materials for the method of the invention may be selected from ores, concentrates, scraps, leach residues and refractory gold materials, which refractory gold materials have been pretreated by pressure oxidation, roasting and/or bacterial leaching. The gold-bearing raw materials used as the starting material in the present invention may also contain silver.
Typically, the starting materials for the method of the invention may be selected from free-milling gold ores/concentrates and pretreated refractory gold concentrates.
Free-milling gold ores/concentrates refer to materials, from which gold can be recovered using cyanide leaching or physical separation methods. Free-milling materials can be sulfidic or oxidic ores. The main minerals of sul-fidic ores are pyrite and pyrrhotite. The oxidic ores mainly contain silicates and ferric/ferrous oxides.
Refractory gold concentrates refer to materials, wherein the gold recovery in conventional cyanide leaching process is less than 80%. In most refractory gold concentrate materials, gold is associated with sulphide minerals as very fine inclusions or as invisible gold in the mineral lattice. Decomposition of gold-bearing minerals is required for gold liberation. Examples of refractory gold concentrates are ores based on arsenopyrite, pyrite and/or silicate.
The pretreatment of the refractory gold concentrates used as the starting material may be performed by a method selected from pressure oxidation, bioleaching and roasting, preferably pressure oxidation.
In one embodiment of the invention, the gold-bearing raw materials used as the starting material are selected from refractory gold concentrates which have been pretreated by pressure oxidation.
Method
In the gold leaching step (a), the gold-bearing raw material is subjected to oxidative chloride leaching in an aqueous leaching liquor in the following conditions: (i) the aqueous leaching liquor contains dissolved cupric ions (Cu2+), chloride (Cl') and bromide (Br'), (ii) pH is within a range wherein the cupric ion does not precipitate, (iii) the oxidation potential is at least 450 mV Pt vs. Ag/AgCI, to provide a gold-containing solution.
In the leaching also silver may be leached and therefore the gold-containing solution may optionally further contain silver.
Typically the method further comprises a liquid/solid separation step (b), wherein the gold-containing solution is separated from the undissolved solid material; a gold recovery step (c), wherein gold is recovered from the gold-containing solution from step (b) to obtain a gold-bearing organic solution and a gold-depleted leach solution containing Cu2+, Cl' and Br', and optionally a circulation step (d), wherein the gold-depleted leach solution containing Cu2+, Cl' and Br' is circulated to the leaching step (a).
The oxidative chloride leaching is typically performed at atmospheric pressure. Further, the oxidative chloride leaching is typically performed at the temperature of at least 50°C, more typically at the temperature of 88 -100°C.
In the oxidative chloride leaching the pH value, i.e. the range wherein the cupric ion does not precipitate, is less than 2.6, typically less than 2.2.
The oxidative chloride leaching is typically performed by providing an oxidizing source into the chloride leaching liquor. Typically, the oxidizing source is an oxygen feed, an oxygen-enriched air feed or an air feed to the solution. The purpose of the oxidizing source is to allow the copper in the solution to maintain in a 2+ ion form.
The oxidation potential is typically 450 - 800 mV Pt vs. Ag/AgCI, typically 450 - 700 mV Pt vs. Ag/AgCI.
In the leaching step, the gold ore/concentrate is introduced into the leaching liquor, which contains Cu2+, Cl' and Br', typically in the following concentrations: 10 - 110 g/l Cu2+, 50-300 g/l Cl' and 1-100 g/l Br (expressed as NaBr). Typically the leaching liquor is aqueous. Furthermore, the leaching liquor as a rule contains acid, in a typical concentration of 5-20 g/l HCI. Typically, oxygen is fed into the leaching liquor. Copper (Cu2+) is required to provide high oxidation power in order that gold can be oxidized together with the oxygen feed. Chloride and bromide (Cl' and Br ) form aqua complexes with gold so that gold is dissolved in the leaching solution. The presence of Br' in the leaching liquor enables to maintain gold in a stabile form in the liquor, in other words the presence of Br' enables the formation of a more stable complex of gold compared to if only Cl' was present. pH of the leaching liquor is kept at a level wherein the cupric ion does not precipitate. Typically the pH of the leaching liquor is less than 2.6, more typically less than 2.2. In one embodiment of the invention, the pH is less than 2.2 but higher than 1.5. It was found that only about 0.5 hours may be sufficient for gold dissolution for example from oxide-based free-milling materials and from refractory concentrates pretreated by pressure oxidation.
In a typical embodiment of the invention, the leaching liquor containing Cu2+, Cl' and Br' is circulated gold-depleted and optionally silver-depleted leach solution obtained from subsequent steps of the method after the recovery of gold and after optional recovery of silver. Before introducing the circulated leaching solution into the leaching step, the solution is as a rule subjected to evaporation to remove excess water. The evaporated leaching solution may be introduced to the leaching as such or, if necessary, after optional regeneration. In the regeneration, the circulated leaching solution is supplemented with fresh leaching chemicals (make-up chemicals) containing Cu2+, Cl' and Br'.
The addition of the make-up chemicals is suitably performed in connection with the leaching.
The leaching provides a gold-containing solution with a gold yield of more than 70%, preferably more than 85%, still more preferably more than 95% and even more than 98% and up to 99.7% based on solid analysis. In addition to gold, the leach solution as a rule contains silver and other components, such as e.g. arsenic, aluminium, iron, cobalt, nickel, and magnesium.
In the liquid/solid separation step (b), the gold-containing solution is separated from the solid material. The solid/liquid separation may be performed by filtering, solid/liquid settling, evaporation or centrifugation, for example.
The gold-containing solution is introduced into the gold recovery step (c), after optional washing.
The gold recovery step (c) may be performed by solvent extraction. The solvent extraction is performed by using an extraction agent, which is selective for gold. In one embodiment of the invention, the solvent extraction is performed by using a diester of 2,2,4-trialkyl-1,3-pentanediol as the extraction agent. The extraction with the diester of 2,2,4-trialkyl-1,3-pentanediol may be performed using the method disclosed in WO 2011/154603 A1. It was found that even 99.9% gold recovery was achieved.
Gold can be stripped from the gold-bearing organic solution obtained in step (c) to obtain an aqueous gold-bearing solution. Water or an aqueous salt solution may be used as the stripping agent.
Furthermore, the method may comprise a further gold recovery step, wherein gold is recovered from the aqueous gold-bearing solution obtained above or even directly from the organic gold-bearing solution obtained in step (c). The further gold recovery step may be performed by a method selected from reduction with oxalic acid, ascorbic acid or glucose, adsorption on activated carbon, cementation and direct burning of gold bearing organic reagent. In one embodiment of the invention, the reduction of gold is performed with oxalic acid.
In the circulation step (d), the gold-depleted leach solution from step (c) containing Cu2+, Cl' and Br' is circulated to the leaching step (a) after optional regeneration and/or after evaporation for removing excess water. Due to the efficient circulation and optional regeneration of the gold-depleted leach solution, accumulation of impurities disturbing gold dissolution is avoided.
In one embodiment of the invention, the method further comprises a silver recovery step, where silver is recovered from at least part of the gold-depleted leach solution obtained from the gold recovery step (c). The silver recovery may be performed by a method selected from solvent extraction and precipitation. In one embodiment of the invention, the silver recovery comprises solvent extraction with Cyanex 471X (a commercial solvent extraction reagent where the active component is triisobutylphosphine sulphide), stripping with an aqueous thiosulfate salt solution, such as sodium thiosulfate solution, and cementation with metall powder, such as Cu powder. For the solvent extraction, Cyanex 471X is typically used as a 0.1-0.7 mol/l solution in a hydrocarbon solvent. The solution may also contain a modifier. The silver recovery may also be performed by sulphide precipitation. Silver is typically recovered with a yield of more than 70%.
In one embodiment of the invention, the gold-depleted leach solution from step (c) is circulated to the leaching step (a) after the silver recovery step.
In the following, the invention is illustrated by referring to Figure 1, which is an exemplary embodiment of the invention where gold leaching is combined with gold recovery and further with silver recovery. A gold concentrate (Au concentrate 5) is introduced into leaching 10, together with oxygen feed 7 and a leaching solution containing Cu (Cu2+),CI' and Br'. In the leaching 10, gold is solubilized forming a gold-containing solution. Leaching is followed by solid/liquid separation (S/L separation 20), where the gold-containing solution is separated from the undissolved solid material (leach residue 105).
The gold-containing solution obtained from the leaching is introduced into gold extraction (Au extraction 30), which produces a gold-bearing organic solution and a gold-depleted leach solution containing Cu2+, Cl' and Br'. The gold-bearing organic solution is further introduced into gold stripping (Au stripping 40), where gold is stripped with water from the gold-bearing organic solution to obtain an aqueous gold-bearing solution. Gold is finally recovered as elemental gold from the aqueous gold-bearing solution by reduction with sodium oxalate (Na oxalate 45) by introducing the aqueous gold-bearing solution to reduction (Au reduction 50). The reduction product is subjected to solid/liquid separation (S/L separation 60), from which gold is recovered as a solid product (Au product 65). The liquid product from the solid/liquid separation contains some impurities, such as iron and copper. The impurities are removed from the solution (effluent treatment 70) by hydroxide precipitation. The slurry from the effluent treatment is introduced into solid/liquid separation (S/L separation 80), from which a hydroxide precipitate 85 and a solution bleed 90 are obtained.
The gold-depleted solution containing Cu2+, Cl' and Br' from Au extraction 30 is introduced into silver recovery, comprising silver extraction (Ag extraction 100), silver stripping (Ag stripping 110), silver cementation with Cu-powder 125 (Ag cementation 120) and solid/liquid separation (S/L separation 130), from which a solid silver product (Ag product 135) is obtained. The liquid product from the solid/liquid separation 130 is introduced into effluent treatment 70 (together with the liquid product from gold recovery).
Part of the leaching solution containing Cu2+, Cl' and Br' from the silver extraction 100 is introduced into evaporation 160 to remove excess water as steam 165. After evaporation to a suitable consistency, the remaining solution 170 containing Cu2+, Cl" and Br" is circulated to leaching 10. A small part of the solution from the silver extraction is introduced into effluent treatment 140, where some impurity metals such as zinc and lead are removed by hydroxide precipitation. The effluent treatment is followed by solid/liquid separation (S/L separation 150). The liquid product from the solid/liquid separation is introduced into evaporation 160. The solid product from the solid/liquid separation is recovered as a Cu-Zn precipitate 155.
The invention relates also to a process arrangement for recovering gold and silver from gold-bearing raw material, wherein the arrangement comprises (a) a gold leaching unit adapted for subjecting the gold-bearing raw material to oxidative chloride leaching in a leaching liquor containing cupric ions(Cu2+), chloride (Cl) and bromide (Br), for dissolving gold and silver, (b) a liquid/solid separation unit, adapted for separating the gold- and silver-containing solution from the undissolved solid material; (c1) a gold recovery unit, adapted for recovering the gold from the gold- and silver-containing solution from unit (b) to obtain a gold-bearing organic solution and a gold-depleted leach solution ; (c2) a silver extraction unit adapted for recovering the silver from the gold-depleted leach solution, and (d) a circulation unit (d), adapted for circulating the gold-depleted leach solution containing Cu2+, Cl' and Br' to the leaching unit (a).
Optionally the process arrangement comprises an evaporation unit adapted for evaporating excess water and an effluent treatment unit for treating liquid obtained from silver extraction unit.
The liquid-solid separation unit may be selected from filter, sol-id/liquid settler, evaporator or centrifuge, for example.
EXAMPLES
The following examples illustrate the invention without limiting the invention in any way.
In the following examples 1-3, leaching tests with different gold concentrates were carried out in order to see whether it is possible to obtain as high extraction of gold with chloride leaching as with cyanide leaching.
Example 1
Recovery of gold from a sulfidic gold concentrate
The sulfidic gold concentrate used as the starting material was a free-milling concentrate. In the concentrate, most of the gold exists as pure metal and it can be dissolved directly with cyanide. The amount of liberated gold in the material is 80.85%. The material contains also locked gold.
Chemical composition of the sulfidic concentrate is presented in
Table 1.
Chloride-bromide leaching test conditions are presented in Table 2. The redox potential varied between 550-676mV Pt vs. Ag/AgCI.
Furthermore, the effect of copper concentration on gold dissolution was studied in test 3. During the test, the copper concentration was increased step by step. Used copper concentrations were 50 g/l, 67 g/l, 83 g/l, and 100 g/l. Addition of copper was made every two hours.
The copper concentration affected gold dissolution. 50 g/l copper dissolved part of gold in half hour (Figure 2). Higher copper concentrations increased gold dissolution.
Additionally, the effect of bromide concentration on gold dissolution was studied in test 4. The sodium bromide concentration was changed every second hours. The sodium bromide concentration effected dissolution of gold (Figure 3). Kinetics of gold dissolution was faster with higher bromide concentrations.
Relatively good extractions of gold (83.9%) were obtained with chloride-bromide leaching. Kinetics was fast.
Example 2.
Recovery of gold from a silicate based gold ore
The silicate based gold ore used as the starting material was also a free-milling ore.
The chemical analyses of the ore is presented in Table 4.
Chloride-bromide leaching test conditions are presented in Table 5. The redox potential varied between 450 - 682 mV Pt vs. Ag/AgCI. A cyanide leaching test for comparison purposes was carried out in the following conditions: solid concentration 33w-%, pH 11, air feed 500 ml/min, NaCN concentration 3 g/l, and leaching time 24 h.
The results from all tests are presented in Table 6.
Furthermore, the gold concentration of the solution vs. leaching time is presented in Figure 4.
In test 3, the effect of copper concentration was also studied. During the leaching, copper concentration had to be so high that redox potential is over 450 mV Pt vs. Ag/AgCI. Copper concentration was increased step by step from 0 g/l to 75 g/l during the test. Used concentrations were 0, 1, 10, 30, 60, and 75 g/l. It seems that 10 g/l copper was a sufficiently high concentration for gold dissolution (Figure 5). Required copper concentration depends on the mineralogy of feed material.
Additionally, the effect of sodium bromide concentration on gold dissolution was studied in test 4 (Figure 6). Used sodium bromide concentrations were 0, 1,5, 10, 40, and 60 g/l.
Furthermore, the effect of chloride concentration on gold dissolution was studied (Figure 7). Chloride concentration 100 g/l increased dissolution of gold. 25 g/l chloride dissolved some of the gold, but most of gold remained in solid. Leaching of gold needed quite high chloride concentrations. According to the test 5, a suitable chloride concentration would be at least 125 g/l for this material. Extraction of gold was 99.98%.
Results of the cyanide leaching test are presented in Figure 8. Extraction of gold was 98.0% for the used silicate based gold ore.
During the leaching tests it was found that the mineral composition of the material as well as copper, bromide, chloride and acid concentrations affect the gold leaching. Relatively good extractions of gold (over 95%, Table 6) were obtained with chloride-bromide leaching. Kinetics was fast in chloride- bromide leaching. In cyanide leaching, the retention time was 24 hours. After 25 hours, the extraction of gold was 98%.
The chloride leaching was possible with low copper and sodium bromide concentrations. The temperature needs to be at least 90°C.
Example 3.
Recovery of gold from pretreated refractory gold concentrate
In the used concentrate, most of the gold is inside sulfide minerals. The chemical composition of the used refractory gold concentrate before pretreatment is presented in Table 7. The gold is mostly locked in pyri-te.
Chloride-bromide leaching test conditions are presented in Table 8. The redox potential varied between 568 - 681 mV Pt vs. Ag/AgCI. In tests 1 - 2, the material was pretreated with POX (pressure oxidation). POX treatments were made in the following conditions: solid concentration was 150 - 300 g/l, temperature was 210°C, and the oxygen overpressure was 6 bar (total pressure was about 26 bar). After POX treatment, hot cure treatment was done. The temperature was decreased to 90°C and the overpressure was released (to atmospheric pressure).
The chloride-bromide leaching results are presented in Table 9.
Relatively good extractions of gold (over 99%) and silver (about 97%) were obtained with chloride-bromide leaching for POX treated material. In test 2 (Figure 9), the effect of sodium bromide concentration was also studied. Sodium bromide concentration did not affect gold extraction in the sodium bromide concentration range used in this case. In Figure 9, the gold concentration of the solution varied widely depending on solid concentration and the amount of solid.
It will be obvious to a person skilled in the art that, as the technology advances, the inventive concept can be implemented in various ways. The invention and its embodiments are not limited to the examples described above but may vary within the scope of the claims.

Claims (25)

1. Menetelmä kultaa sisältävän liuoksen valmistamiseksi kultapitoisista raaka-aineista, missä menetelmä käsittää (a) kullan uuttovaiheen, missä kultapitoinen raaka-aine saatetaan hapettavaan kloridiuuttoon vesipitoisessa uuttoliuoksessa seuraavissa olosuhteissa: (i) vesipitoinen uuttoliuos sisältää liuenneita kupari-ioneita (Cu2+), kloridia (CT) ja bromidia (Br ), (ii) pH on sellaisen vaihteluvälin sisällä, missä kupari-ioni ei saostu, (iii) hapetuspotentiaali on vähintään 450 mV Pt vs. Ag/AgCI kultaa sisältävän liuoksen, joka mahdollisesti sisältää lisäksi hopeaa, aikaansaamiseksi, (b) neste-kiintoaine-erotusvaiheen, missä kultaa sisältävä liuos erotetaan liukenemattomasta kiintoaineesta; (c) kullan talteenottovaiheen, missä kultaa otetaan talteen vaiheesta (b) saadusta kultaa sisältävästä liuoksesta kultapitoisen orgaanisen liuoksen ja kullan suhteen köyhtyneen uuttoliuoksen, joka sisältää aineita Cu2+, Cl' ja Br', saamiseksi; ja (c’) haihdutusvaiheen, missä vaiheesta (c) saatua kullan suhteen köyhtynyttä uuttoliuosta, joka sisältää aineita Cu2+, Cl' ja Br', haihdutetaan ylimääräisen veden poistamiseksi; ja (d) kierrätysvaiheen, missä haihdutusvaiheesta saatua kullan suhteen köyhtynyttä uuttoliuosta, joka sisältää aineita Cu2+, Cl' ja Br', kierrätetään uuttovaiheeseen (a).
2. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä kultapitoinen raaka-aine on valittu malmeista, rikasteista, jätteistä, uutto-jäännöksistä ja vaikeasti sulavista kuvamateriaaleista, jotka vaikeasti sulavat kuvamateriaalit on esikäsitelty painehapetuksella, pasutuksella ja/tai bakteeri-uutolla.
3. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä helposti käsiteltäviä kultamalmeja/-rikasteita ja esikäsiteltyjä vaikeasti sulavia kultarikasteita käytetään raaka-aineena ja ne on valittu sulfidisista ja oksi-doituneista materiaaleista.
4. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä kultapitoinen raaka-aine on valittu vaikeasti sulavista kultarikasteista ja raaka-aineena käytettävien vaikeasti sulavien kultarikasteiden esikäsittely on suoritettu menetelmällä, joka on valittu painehapetuksesta, biouutosta ja pasutuk-sesta ja joka on edullisesti painehapetus.
5. Patenttivaatimuksen 4 mukainen menetelmä, missä kultapitoinen raaka-aine on valittu vaikeasti sulavista kultarikasteista, joita on esikäsitelty painehapetuksella.
6. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä hapettava kloridiuutto suoritetaan ilmanpaineessa.
7. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä hapettava kloridiuutto suoritetaan vähintään 50 °C:n lämpötilassa, tyypillisesti 88-100 °C:n lämpötilassa.
8. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä pH-arvo, jolla kupari-ioni ei saostu, on alle 2,6, tyypillisesti alle 2,2.
9. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä hapettava kloridiuutto suoritetaan tarjoamalla käyttöön hapettava lähde.
10. Patenttivaatimuksen 9 mukainen menetelmä, missä hapettava lähde on happisyöte, hapella rikastettu ilmasyöte tai ilmasyöte liuokseen.
11. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä hapetuspotentiaali on 450-800 mV Pt vs. Ag/AgCI, tyypillisesti 450-700 mV Pt vs. Ag/AgCI.
12. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä aineiden Cu2+, Cl'ja Br'pitoisuudet uuttoliuoksessa ovat 10-110 g/l Cu2+, 50-300 g/l Cl'ja 1-100 g/l Br' (ilmaistuna aineena NaBr).
13. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä uuttoliuoksen hapon väkevyys on 5-20 g/l HCI.
14. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä kullan saanto kullan uuttovaiheessa (a) on yli 70 %, edullisesti yli 85 %, edullisemmin yli 95 % ja erityisesti yli 98 %.
15. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä kullan talteenottovaihe (c) suoritetaan liuotinuutolla, edullisesti uuttamalla 2,2,4-trialkyyli-1,3-pentaanidiolin diesterillä.
16. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä menetelmä käsittää lisäksi kullan poistovaiheen (stripping), missä kultaa poistetaan vaiheessa (c) saadusta kultapitoisesta orgaanisesta liuoksesta vesi-ja kultapitoisen liuoksen saamiseksi.
17. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä menetelmä käsittää vielä erään kullan talteenottovaiheen, missä kultaa otetaan talteen patenttivaatimuksen 1 vaiheen (c) kultapitoisesta orgaanisesta liuoksesta tai patenttivaatimuksen 16 vesi-ja kultapitoisesta liuoksesta.
18. Patenttivaatimuksen 17 mukainen menetelmä, missä mainittu vielä eräs kullan talteenottovaihe suoritetaan menetelmällä, joka on valittu pelkistyksestä oksaalihapolla, askorbiinihapolla tai glukoosilla, adsorptiosta aktiivihiileen, kultapitoisen orgaanisen reagenssin sementoinnista ja suorasta poltosta.
19. Jonkin edellisen patenttivaatimuksen mukainen menetelmä, missä menetelmä käsittää lisäksi hopean talteenottovaiheen, missä hopeaa otetaan talteen ainakin osasta kullan suhteen köyhtyneestä uuttoliuosta, joka on saatu kullan talteenottovaiheesta (c).
20. Patenttivaatimuksen 19 mukainen menetelmä, missä hopean talteenottovaihe käsittää menetelmän, joka on valittu liuotinuutosta ja saostuksesta.
21. Patenttivaatimuksen 20 mukainen menetelmä, missä hopean talteenottovaihe käsittää liuotinuuton aineella Cyanex 471X (tri-isobutyyIifos-fiinisulfidi), poiston (stripping) vesipitoisella tiosulfaattisuolaliuoksella ja hopean sementoinnin tiosulfaattiliuoksesta metallijauheella.
22. Patenttivaatimuksen 20 mukainen menetelmä, missä hopean talteenottovaihe käsittää sulfidin saostuksen.
23. Patenttivaatimuksen 19 mukainen menetelmä, missä vaiheesta (c) saatua kullan suhteen köyhtynyttä uuttoliuosta palautetaan uuttovaihee-seen (a) hopean talteenottovaiheen jälkeen.
24. Jonkin patenttivaatimuksen 19-23 mukainen menetelmä, missä hopeaa otetaan talteen yli 70 %:n saannolla.
25. Prosessijärjestely kullan ja hopean talteen ottamiseksi kultapitoisesta raaka-aineesta, missä järjestely käsittää (a) kullan uuttoyksikön, joka on sovitettu saattamaan kultapitoinen raaka-aine hapettavaan kloridiuuttoon uuttoliuoksessa, joka sisältää kupari-ioneita (Cu2+), kloridia (Cl') ja bromidia (Br ), kullan ja hopean liuottamiseksi, (b) neste-kiintoaine-erotusyksikön, joka on sovitettu kultaa ja hopeaa sisältävän liuoksen erottamiseksi liukenemattomasta kiintoaineesta; (c1) kullan talteenottoyksikön, joka on sovitettu kullan talteen ottamiseksi yksiköstä (b) saadusta kultaa ja hopeaa sisältävästä liuoksesta kultapitoisen orgaanisen liuoksen ja kullan suhteen köyhtyneen uuttoliuoksen saamiseksi; (c2) hopean uuttoyksikön, joka on sovitettu hopean talteen ottamiseksi kullan suhteen köyhtyneestä uuttoliuoksesta; (c3) haihdutusyksikön, joka on sovitettu ylimääräisen veden haihduttamiseksi, ja effluentin käsittely-yksikön hopean uuttoyksiköstä saadun nesteen käsittelemiseksi; ja (d) kierrätysyksikön, joka on sovitettu kullan suhteen köyhtyneen uuttoliuoksen, joka sisältää aineita Cu2+, Cl' ja Br', kierrättämiseksi uuttoyksik-köön (a).
FI20135448A 2013-04-30 2013-04-30 Menetelmä kultaa sisältävän liuoksen valmistamiseksi ja prosessijärjestely kullan ja hopean talteenottamiseksi FI124954B (fi)