CN1397626A - 防尘固沙水基粘接剂及制备方法 - Google Patents
防尘固沙水基粘接剂及制备方法 Download PDFInfo
- Publication number
- CN1397626A CN1397626A CN 02104481 CN02104481A CN1397626A CN 1397626 A CN1397626 A CN 1397626A CN 02104481 CN02104481 CN 02104481 CN 02104481 A CN02104481 A CN 02104481A CN 1397626 A CN1397626 A CN 1397626A
- Authority
- CN
- China
- Prior art keywords
- water
- sand
- emulsion
- base
- base adhesive
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
本发明涉及防尘固沙水基粘接剂及制备方法,其特征在于物理黏结的原理,高分子水基树脂/乳液为主剂配制的水基粘接剂,经喷洒到沙土表面,水份挥发后,靠大分子将沙土粘接在一起。没有化学过程,不产生低分子物,不含重金属元素,粘接剂为中性,对植物生长和水质、土质无影响。下雨的雨水可以慢慢地渗下。同时,减少地下水的蒸发速度,起到水土保持的作用。特别是对北方和西部缺水地区,具有广泛的应用空间。
Description
技术领域
本发明属于化工类粘接剂技术领域,应用于环境保护产业的固尘固沙。本发明还涉及物理固沙固尘技术和水基粘接剂的配方。
技术背景
本发明涉及的水基粘接剂,不含对环境水质、土质污染的重金属元素、有机溶剂等,不产生二次污染。
在本发明之前,国内外均采用化学固沙固尘的方法,所用的粘接剂含有对水土有害的表面活性剂、乳化剂、沥青分解物等,对植物生长和水土保持不利。
发明内容
本发明的特点在于物理粘接的原理,高分子水基树脂/乳液为主剂配制的水基粘接剂,经喷洒到沙土表面,水份挥发后,靠大分子将沙土粘接在一起。没有化学过程,不产生低分子物,不含重金属元素,粘接剂为中性,对植物生长和水质、土质无影响。下雨的雨水可以慢慢地渗下。同时,减少地下水的蒸发速度,起到水土保持的作用。特别是对北方和西部缺水地区,具有广泛的应用空间。
本发明通过下述技术方案实现:
防尘固沙水基粘接剂,其特征是水基树脂/乳液加入羧乙基纤维素和成膜助剂,按下述重量份配比:
水基树脂/乳液5-53 羧乙基纤维素3-10
成膜助剂1-8 PH值调节剂1-4
自来水20-60
其中水基树脂可以是水基丙烯酸树脂、水基聚酰胺树脂和水基硅丙树脂。乳液可以是苯乙烯-丙烯酸乳液、纯丙烯酸乳液、有机硅-丙烯酸乳液和乙丙乳液。
其中成膜助剂可以是乙二醇笨醚、丙二醇笨醚。
防尘固沙水基粘接剂的制配方法,按下述步骤进行:
将羧乙基纤维素配制成百分之一的水溶液,将自来水、成膜助剂、羧乙基纤维素水溶液、PH值调节剂在均匀搅拌条件下,加入水基树脂/乳液,所有的材料加完后,继续搅拌30分钟后,过滤,检查、调节酸碱度。
本发明的防尘固沙水基粘接剂具有如下技术性能:
黏度,(涂4杯):15-35秒
干燥时间,23℃,RH 55%
表干时间:2小时
实干时间:24小时
柔韧性:2毫米
黏结强度,(纱布/纱布):35N/CM2
吹风重量损失(风速20M/秒):≤5%
重金属元素含量:0%
储存时间:6个月
具体实施方式
实施例1
水基丙烯酸树脂:25 羧乙基纤维素水溶液:6
乙二醇笨醚:5 水基PH值调节剂:2
自来水:58
实施例2
水基聚酰胺树脂:25 羧乙基纤维素水溶液:6
乙二醇笨醚:5 水基PH值调节剂:2
自来水:58
实施例3
水基有机硅丙烯酸树脂:25 羧乙基纤维素水溶液:6
乙二醇笨醚:5 水基PH值调节剂:2
自来水:58
实施例4
纯丙乳液:39 羧乙基纤维素水溶液:6
乙二醇笨醚:5 水基PH值调节剂:2
自来水:48
实施例5
苯丙乳液:39 羧乙基纤维素水溶液:6
乙二醇笨醚:5 水基PH值调节剂:2
自来水:48
实施例6
硅丙乳液:39 羧乙基纤维素水溶液:6
乙二醇笨醚:5 水基PH值调节剂:2
自来水:48
实施例7
乙丙乳液:39 羧乙基纤维素水溶液:6
丙二醇笨醚:5 水基PH值调节剂:2
自来水:48
实施例8
纯丙乳液:39 羧乙基纤维素水溶液:6
丙二醇笨醚:5 水基PH值调节剂:2
自来水:48
Claims (5)
- 防尘固沙水基粘接剂及制备方法1 防尘固沙水基粘接剂及制备方法,其特征在于用物理过程的方法,按下述重量份配比制成的没有环境污染的水基粘接剂:高分子水基树脂/乳液5-53 羧乙基纤维素3-10成膜助剂1-8 PH值调节剂1-4自来水20-60
- 2 权利要求1所述的防尘固沙水基粘接剂,其特征在于所述的高分子水基树脂/乳液为水基丙烯酸树脂、水基聚酰胺树脂和水基硅丙树脂。乳液可以是苯乙烯-丙烯酸乳液、纯丙烯酸乳液、有机硅-丙烯酸乳液和乙丙乳液。
- 3 权利要求1所述的防尘固沙水基粘接剂及制备方法,其特征为物理过程,无化学反应,制备过程无环境污染。
- 4 根据权利要求1所述的防尘固沙水基粘接剂,其特征在于固尘固沙施工过程无环境污染。
- 5 根据权利要求1所述的防尘固沙水基粘接剂,其特征在于无重金属元素,对水质、土质无二次污染。