CN1197912C - Method for mfg of jade imitated material - Google Patents

Method for mfg of jade imitated material Download PDF

Info

Publication number
CN1197912C
CN1197912C CN 03125217 CN03125217A CN1197912C CN 1197912 C CN1197912 C CN 1197912C CN 03125217 CN03125217 CN 03125217 CN 03125217 A CN03125217 A CN 03125217A CN 1197912 C CN1197912 C CN 1197912C
Authority
CN
China
Prior art keywords
jade
unsaturated polyester
ketone peroxide
methylethyl ketone
green
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN 03125217
Other languages
Chinese (zh)
Other versions
CN1483762A (en
Inventor
蒙瑞基
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Guangxi Lisheng Stone Co ltd
Guangxi Nanning Chengyuan Technology Co ltd
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN 03125217 priority Critical patent/CN1197912C/en
Publication of CN1483762A publication Critical patent/CN1483762A/en
Application granted granted Critical
Publication of CN1197912C publication Critical patent/CN1197912C/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

The present invention relates to a method for making a jade imitated material. Main raw materials, such as aluminium hydroxide, stone powder, glass powder, unsaturated polyester resin cobalt iso-octoate or cobalt naphthenate, methylethyl ketone peroxide, etc. are used. The present intention has the advantages of large proportioning range of each material, easy obtaining of the raw material, simple and mature manufacturing process, shapely and random molding of the product, corrosion resistance, easy cleaning, good flame retardance, no pollution and low manufacturing cost, and can be used for making lines, Rome columns, relief, etc. for building finishing.

Description

The making method of imitative jade material
Technical field
The invention belongs to the making method of artificial jade stone material.
Background technology
Attractive in appearance, durable, pollution-free for finishing material, particularly constructional ornamental material can be satisfied simultaneously, and low-cost requirement, the technology of many rostones has appearred, and the instrument artificial jade just has multiple production method.Chinese patent application " manufacture method and the goods of imitative stone material " (application number 02103809.0), " a kind of artificial jade and woodwork inlay " (application number 97114408.7), " artificial jade " (application number 91101451.9) etc. all belong to the making category of rostone.But the manufacture craft that these technology have is complicated, the cost height; The making raw material sources that have are limited, and price is also high; So still constantly there is the new technology of making various rostones to occur.
Summary of the invention
The technical problem to be solved in the present invention be adopt the raw material that is easy to get, simplify production technique, obtain at lower cost that product surface is smooth, the artificial jade of hard pliable and tough, corrosion-resistant, fire-resistant, the anti-distortion of endoplasm.
The making method of imitative jade material provided by the invention is to solve the problems of the technologies described above with following technical scheme: this jade material is made by aggregate, tackiness agent and auxiliary material, above-mentioned materials mixed and fully stir after curing molding at room temperature, it is characterized in that each composition and weight part thereof are as follows
Aggregate 50-105
Unsaturated polyester resin 19-30
Different Rinmann's green 0.05-0.5
Methylethyl ketone peroxide 0.05-0.8
Mill base 0-0.2
Described aggregate is a kind of in aluminium hydroxide, stone flour, the glass powder or their mixture.
The making prescription of imitative jade is: (weight part, as follows)
1. aluminium hydroxides 68~80 of filling a prescription
Unsaturated polyester resin 19~30
Different Rinmann's green 0.05~0.5
Methylethyl ketone peroxide 0.05~0.8
Mill base 0~0.2
2. stone flours 60~75 of filling a prescription
Unsaturated polyester resin 19~30
Different Rinmann's green 0.05~0.5
Methylethyl ketone peroxide 0.05~0.8
Mill base 0~0.2
3. aluminium hydroxides 51~70 of filling a prescription
Stone flour 10~30
Unsaturated polyester resin 20~30
Different Rinmann's green 0.05~0.5
Methylethyl ketone peroxide 0.05~0.8
Mill base 0~0.2
4. aluminium hydroxides 30~50 of filling a prescription
Glass powder 20~40
Unsaturated polyester resin 19~30
Different Rinmann's green 0.05~0.5
Methylethyl ketone peroxide 0.05~0.8
Mill base 0~0.2
5. aluminium hydroxides 10~25 of filling a prescription
Stone flour 40~50
Glass powder 10~30
Unsaturated polyester resin 19~30
Different Rinmann's green or alkane naphthenic acid cobalt 0.05~0.5
Methylethyl ketone peroxide 0.05~0.8
Mill base 0~0.2
6. stone flours 55~70 of filling a prescription
Aluminium hydroxide 10~20
Unsaturated polyester resin 19~30
Different Rinmann's green or alkane naphthenic acid cobalt 0.05~0.5
Methylethyl ketone peroxide 0.05~0.8
Mill base 0~0.2
Produce imitative jade material with method of the present invention, raw material is easy to get, technical maturity, and simple, handsome in appearance, random, product is corrosion-resistant, easy cleaning, good flame resistance, pollution-free, and cost of manufacture is very low.
Embodiment
Make imitative jade material with method of the present invention, can adopt different composition of raw materials, when for example needing to make the bigger ornament of transparency, can be equipped with many aluminium hydroxide in the imitative jade raw material according to different needs; When need making the higher ornament of hardness, the stone flour in the raw material can account for higher proportion; Adding glass powder can make in the ornament body sparkling particulate etc.The present invention has adopted the prior art of making binding agent with unsaturated polyester resin, and does promotor with different Rinmann's green, and methylethyl ketone peroxide is made solidifying agent.When making ornament, if each raw material prepared by desired product character and mixing after die casting, solidifying formation, the demoulding, after surface treatment finished product.
Can make the multiple product of imitating jade with method of the present invention, as various mouldings, FRP Columns, embossment and various artworks etc.
Embodiment 1:
After 1.5 kilograms of 196# unsaturated polyester resins, 3.7 kilograms in aluminium hydroxide (toothpaste level), 0.003 kilogram of different Rinmann's green, the abundant stirring of 0.003 kilogram of mixing of methylethyl ketone peroxide, insert and place indoor curing in the lines mould that coats releasing agent naturally, the demoulding after the moulding promptly gets after benefit is filled out bubble and imitates jade finishing lines.
Embodiment 2:
After 1.08 kilograms of 128# unsaturated polyester resins, 2.513 kilograms of calcite stone flours, 0.003 kilogram of black color paste, 0.002 kilogram of different Rinmann's green, the abundant stirring of 0.002 kilogram of mixing of methylethyl ketone peroxide, insert in the lines mould that coats releasing agent, curing molding, the demoulding in 36 ℃ room temperature promptly get the imitative jade lines of black after benefit is filled out bubble.
Embodiment 3:
With 6 kilograms in 191# unsaturated polyester resin 2.06kg, aluminium hydroxide, 2 kilograms of rhombspar stone flours, 0.021 kilogram of green mill base, 0.01 kilogram of different Rinmann's green, methylethyl ketone peroxide mix fully for 0.082 kilogram inserts the curing molding demoulding at room temperature in the animal mould that coats releasing agent after the stirring, after benefit promptly gets the imitative jade finished product of animal shape after filling out bubble.
Embodiment 4:
With 3.2 kilograms of 128# unsaturated polyester resins, 4.6 kilograms in aluminium hydroxide, 3.6 kilograms in glass powder, 0.055 kilogram of different Rinmann's green, 0.06 kilogram of methylethyl ketone peroxide, 0.005 kilogram of BigBlue mill base, mix fully and insert the curing molding demoulding at room temperature in the turriform mould that coats releasing agent after the stirring, after benefit promptly gets the imitative jade finished product of turriform after filling out bubble.
Embodiment 5:
With 32 kilograms of stone flours, 10 kilograms in aluminium hydroxide, 13 kilograms in glass powder, 0.2 kilogram of different Rinmann's green, 0.2 kilogram of methylethyl ketone peroxide, 13 kilograms of unsaturated polyester resins, 0.01 kilogram of beige mill base, mix also and fully insert in the FRP Columns mould that coats releasing agent after the stirring, curing and demolding, use in proportion slurry with two semicolumn joint closes again, wait after the curing the imitative jade FRP Columns of beige.
Embodiment 6:
After 110 kilograms of stone flours, 22 kilograms in aluminium hydroxide, 41 kilograms of unsaturated polyester resins, 0.4 kilogram of different Rinmann's green, 0.3 kilogram of mixing of methylethyl ketone peroxide and fully stirring, insert coat releasing agent, in be carved with the Kowloon and play with water in the mould of pattern, under natural temperature, solidify, mend after the demoulding and fill out bubble, promptly get and imitate the jade Kowloon embossment of playing with water.

Claims (1)

1. the making method of an imitative jade material, this jade material is made by aggregate, tackiness agent and auxiliary material, above-mentioned materials is mixed and fully stir after curing molding at room temperature, it is characterized in that each composition and weight part thereof are as follows:
Aggregate 50-105
Unsaturated polyester resin 19-30
Different Rinmann's green 0.05-0.5
Methylethyl ketone peroxide 0.05-0.8
Mill base 0-0.2
Described aggregate is a kind of in aluminium hydroxide, stone flour, the glass powder or their mixture.
CN 03125217 2003-07-31 2003-07-31 Method for mfg of jade imitated material Expired - Fee Related CN1197912C (en)