CN109439928A - The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process - Google Patents
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process Download PDFInfo
- Publication number
- CN109439928A CN109439928A CN201811340116.4A CN201811340116A CN109439928A CN 109439928 A CN109439928 A CN 109439928A CN 201811340116 A CN201811340116 A CN 201811340116A CN 109439928 A CN109439928 A CN 109439928A
- Authority
- CN
- China
- Prior art keywords
- magging
- zinc
- novel environment
- friendlymaterial material
- production method
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The present invention relates to wet processes to practice zinc technical field, and in particular to the production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process;The following steps are included: basic zinc carbonate is slowly added to synthesize in hydrofluoric acid, the performance improving agent and activator prepared in advance are added simultaneously, synthesize the slurry of de-magging Novel environment-friendlymaterial material, by being dehydrated, being dried, de-magging Novel environment-friendlymaterial material can be obtained, filtrate, which returns, prepares hydrofluoric acid recycling;It is capable of selectivity the magnesium precipitate in zinc electrolyte gets off, and reduces environmental pollution.
Description
Technical field
The present invention relates to wet processes to practice zinc technical field, and in particular to de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process
Production method.
Background technique
In the production of zinc refining, 80% or more is accounted for using Zinc hydrometallurgy process.The raw material zinc sulphide of wet zinc-making system
Magnesium in concentrate and partial supplementary material constantly enters system, and recycles and be enriched in wet zinc-making system, if do not taken effectively
Measure, content of magnesium can be continuously increased in system, can reach 40g/L or more so that magnesium be easy in the lower pipeline of temperature or
Chamber wall crystallization improves blocking risk, causes potential threat to zinc abstraction equipment;High magnesium ion concentration will increase solution viscosity,
Current efficiency is reduced in electrolytic process, increases energy consumption;Meanwhile high magnesium ion concentration can reduce the zinc output efficiency of system.Cause
This needs the magnesium that will be enriched in solution to clear out of system, to guarantee the balance of magnesium in zinc abstraction system, it is ensured that zinc electrolysis is smooth
It carries out.
Currently, most common except magnesium method has in wet zinc-making system: crystallisation by cooling method, the heavy zinc row magnesium processes of neutralization etc.,
There is its advantage and disadvantage.The principle of crystallisation by cooling method demagging is the variation based on magnesium salts solubility, when the close saturation of content of magnesium, is adopted
With pressure or Temperature fall, Mg2+Then with MgSO4 Crystallization is precipitated, but in actual operation, often there is a large amount of zinc sulfate,
The salts such as calcium sulfate are precipitated simultaneously, keep demagging effect undesirable, while also resulting in a large amount of losses of zinc.And it neutralizes heavy zinc and arranges magnesium processes
It is that addition lime carries out neutralization precipitation in liquid after electrolysis, is precipitated out zinc, magnesium plasma all from solution, the method is not only
Large quantities of lime is consumed, many waste residues and waste water are generated, while causing the loss and cost recovery raising of a large amount of zinc.
The method of above-mentioned removing magnesium ion, first to recycle zinc as major measure, and zinc can only be with the shape of material containing zinc
Formula recycling, cost recovery is all higher, and the rate of recovery of zinc is also undesirable.Several distinct issues are faced with, first is that the quantity of slag is big, very
The problems such as difficult discharge for fundamentally solving slag, storage and comprehensive utilization;Second is operating cost height;Third is the waste residue generated
The value of comprehensive utilization is low, and long-term environmental protection management difficulty is big, and enterprise's long period steady production can not be supported to run.
Thus, it explores new technique and realizes that the open circuit of magnesium in zinc hydrometallurgy is very important.
Summary of the invention
The purpose of the present invention is to provide a kind of production methods of de-magging Novel environment-friendlymaterial material in Zinc Hydrometallurgy Process, can
Selectivity gets off the magnesium precipitate in zinc electrolyte, and reduces environmental pollution.
In order to solve the above technical problems, the invention adopts the following technical scheme:
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, comprising the following steps: delay basic zinc carbonate
Slow be added in hydrofluoric acid is synthesized, while the performance improving agent A and activator B prepared in advance is added, and synthesizes de-magging Novel ring
By being dehydrated, being dried de-magging Novel environment-friendlymaterial material can be obtained, filtrate returns to preparation hydrofluoric acid and follows in the slurry for protecting material
Ring uses.
Further, the mass percentage concentration of basic zinc carbonate is 57%.
Further, the temperature of Synthesis is 30-80 DEG C.
Further, the mass percentage concentration of hydrofluoric acid is 12-30%.
Further, performance improving agent A 7L and activator B 3L is added in every cube of basic zinc carbonate.
Further, generated time 2-8h.
Compared with prior art, the beneficial effects of the present invention are:
1. de-magging Novel environment-friendlymaterial material of the invention can selectively get off the magnesium precipitate in zinc electrolyte, while to electric zinc system
System will not be brought a negative impact, and just meet the needs of zinc industry development.
2. the zinc-containing solution Returning process after demagging uses, fundamentally solve that domestic demagging at present is expensive and ring
The heavy-polluted problem in border.
Specific embodiment
In order to make the objectives, technical solutions, and advantages of the present invention clearer, with reference to embodiments, to the present invention
It is further elaborated.It should be appreciated that the specific embodiments described herein are merely illustrative of the present invention, it is not used to
Limit the present invention.
Embodiment 1
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, comprising the following steps: delay basic zinc carbonate
Slow be added in hydrofluoric acid is synthesized, while the performance improving agent A and activator B prepared in advance is added, and synthesizes de-magging Novel ring
By being dehydrated, being dried de-magging Novel environment-friendlymaterial material can be obtained, filtrate returns to preparation hydrofluoric acid and follows in the slurry for protecting material
Ring uses, and de-magging Novel environment-friendlymaterial material of the invention can selectively get off the magnesium precipitate in zinc electrolyte, while to electric zinc
System will not be brought a negative impact, and just meet the needs of zinc industry development.
Embodiment 2
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, comprising the following steps: delay basic zinc carbonate
Slow be added in hydrofluoric acid is synthesized, and the mass percentage concentration of basic zinc carbonate is 57%, while the performance prepared in advance is added and changes
It is novel that de-magging can be obtained by being dehydrated, being dried in the slurry of kind agent A and activator B, synthesis de-magging Novel environment-friendlymaterial material
Environment-friendly materials, filtrate, which returns, prepares hydrofluoric acid recycling, and de-magging Novel environment-friendlymaterial material of the invention can be selectively by zinc electricity
Magnesium precipitate in solution liquid gets off, while will not bring a negative impact to electric Zn system, is just meeting the needs of zinc industry development.
Embodiment 3
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, comprising the following steps: delay basic zinc carbonate
Slow be added in hydrofluoric acid is synthesized, while the performance improving agent A and activator B prepared in advance is added, and synthesizes de-magging Novel ring
By being dehydrated, being dried de-magging Novel environment-friendlymaterial material can be obtained, filtrate returns to preparation hydrofluoric acid and follows in the slurry for protecting material
Ring uses, and the temperature of Synthesis is 30 DEG C, and de-magging Novel environment-friendlymaterial material of the invention can selectively will be in zinc electrolyte
Magnesium precipitate gets off, while will not bring a negative impact to electric Zn system, is just meeting the needs of zinc industry development.
Embodiment 4
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, comprising the following steps: delay basic zinc carbonate
Slow be added in hydrofluoric acid is synthesized, while the performance improving agent A and activator B prepared in advance is added, and synthesizes de-magging Novel ring
By being dehydrated, being dried de-magging Novel environment-friendlymaterial material can be obtained, filtrate returns to preparation hydrofluoric acid and follows in the slurry for protecting material
Ring uses, and the temperature of Synthesis is 50 DEG C, and de-magging Novel environment-friendlymaterial material of the invention can selectively will be in zinc electrolyte
Magnesium precipitate gets off, while will not bring a negative impact to electric Zn system, is just meeting the needs of zinc industry development.
Embodiment 5
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, comprising the following steps: delay basic zinc carbonate
Slow be added in hydrofluoric acid is synthesized, while the performance improving agent A and activator B prepared in advance is added, and synthesizes de-magging Novel ring
By being dehydrated, being dried de-magging Novel environment-friendlymaterial material can be obtained, filtrate returns to preparation hydrofluoric acid and follows in the slurry for protecting material
Ring uses, and the temperature of Synthesis is 80 DEG C, and de-magging Novel environment-friendlymaterial material of the invention can selectively will be in zinc electrolyte
Magnesium precipitate gets off, while will not bring a negative impact to electric Zn system, is just meeting the needs of zinc industry development.
Embodiment 6
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, comprising the following steps: delay basic zinc carbonate
Slow be added in hydrofluoric acid is synthesized, while the performance improving agent A and activator B prepared in advance is added, and synthesizes de-magging Novel ring
By being dehydrated, being dried de-magging Novel environment-friendlymaterial material can be obtained, filtrate returns to preparation hydrofluoric acid and follows in the slurry for protecting material
Ring uses, and the mass percentage concentration of hydrofluoric acid is 12%, and the zinc-containing solution Returning process after demagging uses, and fundamentally solves
The domestic problem that demagging is expensive and environmental pollution is big at present.
Embodiment 7
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, comprising the following steps: delay basic zinc carbonate
Slow be added in hydrofluoric acid is synthesized, while the performance improving agent A and activator B prepared in advance is added, and synthesizes de-magging Novel ring
By being dehydrated, being dried de-magging Novel environment-friendlymaterial material can be obtained, filtrate returns to preparation hydrofluoric acid and follows in the slurry for protecting material
Ring uses, and the mass percentage concentration of hydrofluoric acid is 20%, and the zinc-containing solution Returning process after demagging uses, and fundamentally solves
The domestic problem that demagging is expensive and environmental pollution is big at present.
Embodiment 9
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, comprising the following steps: delay basic zinc carbonate
Slow be added in hydrofluoric acid is synthesized, while the performance improving agent A and activator B prepared in advance is added, and synthesizes de-magging Novel ring
By being dehydrated, being dried de-magging Novel environment-friendlymaterial material can be obtained, filtrate returns to preparation hydrofluoric acid and follows in the slurry for protecting material
Ring uses, and the mass percentage concentration of hydrofluoric acid is 30%, and the zinc-containing solution Returning process after demagging uses, and fundamentally solves
The domestic problem that demagging is expensive and environmental pollution is big at present.
Embodiment 9
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, comprising the following steps: delay basic zinc carbonate
Slow be added in hydrofluoric acid is synthesized, while the performance improving agent A and activator B prepared in advance is added, and synthesizes de-magging Novel ring
By being dehydrated, being dried de-magging Novel environment-friendlymaterial material can be obtained, filtrate returns to preparation hydrofluoric acid and follows in the slurry for protecting material
Ring uses, and performance improving agent A 7L and activator B 3L is added in every cube of basic zinc carbonate, and the zinc-containing solution after demagging returns
Process uses, and fundamentally solves the problems, such as that domestic demagging is expensive at present and environmental pollution is big.
Embodiment 10
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, comprising the following steps: delay basic zinc carbonate
Slow be added in hydrofluoric acid is synthesized, while the performance improving agent A and activator B prepared in advance is added, and synthesizes de-magging Novel ring
By being dehydrated, being dried de-magging Novel environment-friendlymaterial material can be obtained, filtrate returns to preparation hydrofluoric acid and follows in the slurry for protecting material
Ring uses, generated time 2h, and the zinc-containing solution Returning process after demagging uses, and fundamentally solves domestic demagging valence at present
The problem that lattice are expensive and environmental pollution is big.
Embodiment 11
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, comprising the following steps: delay basic zinc carbonate
Slow be added in hydrofluoric acid is synthesized, while the performance improving agent A and activator B prepared in advance is added, and synthesizes de-magging Novel ring
By being dehydrated, being dried de-magging Novel environment-friendlymaterial material can be obtained, filtrate returns to preparation hydrofluoric acid and follows in the slurry for protecting material
Ring uses, generated time 5h, and the zinc-containing solution Returning process after demagging uses, and fundamentally solves domestic demagging valence at present
The problem that lattice are expensive and environmental pollution is big.
Embodiment 12
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, comprising the following steps: delay basic zinc carbonate
Slow be added in hydrofluoric acid is synthesized, while the performance improving agent A and activator B prepared in advance is added, and synthesizes de-magging Novel ring
By being dehydrated, being dried de-magging Novel environment-friendlymaterial material can be obtained, filtrate returns to preparation hydrofluoric acid and follows in the slurry for protecting material
Ring uses, generated time 8h, and the zinc-containing solution Returning process after demagging uses, and fundamentally solves domestic demagging valence at present
The problem that lattice are expensive and environmental pollution is big.
Embodiment 13
The production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, comprising the following steps: delay basic zinc carbonate
Slow be added in hydrofluoric acid is synthesized, and the mass percentage concentration of basic zinc carbonate is 57%, and the mass percentage concentration of hydrofluoric acid is
20%, while the performance improving agent A and activator B prepared in advance is added, performance improving agent A is added in every cube of basic zinc carbonate
It is novel that de-magging can be obtained by being dehydrated, being dried in the slurry of 7L and activator B 3L, synthesis de-magging Novel environment-friendlymaterial material
Environment-friendly materials, filtrate, which returns, prepares hydrofluoric acid recycling, and the temperature of Synthesis is 50 DEG C, generated time 5h, the present invention
De-magging Novel environment-friendlymaterial material selectively the magnesium precipitate in zinc electrolyte can be got off, while electric Zn system will not be brought negative
Face is rung, and is just meeting the needs of zinc industry development;Zinc-containing solution Returning process after demagging uses, and fundamentally solves at present
The problem that domestic demagging is expensive and environmental pollution is big.
Although reference be made herein to invention has been described for multiple explanatory embodiments of the invention, however, it is to be understood that
Those skilled in the art can be designed that a lot of other modification and implementations, these modifications and implementations will fall in this Shen
It please be within disclosed scope and spirit.It more specifically, within the scope of the present disclosure and claims, can be to master
The building block and/or layout for inscribing composite configuration carry out a variety of variations and modifications.In addition to what is carried out to building block and/or layout
Outside modification and improvement, to those skilled in the art, other purposes also be will be apparent.
Claims (6)
1. the production method of de-magging Novel environment-friendlymaterial material in a kind of Zinc Hydrometallurgy Process, it is characterised in that: the following steps are included: will
Basic zinc carbonate is slowly added to be synthesized in hydrofluoric acid, while the performance improving agent A and activator B prepared in advance is added, and closes
De-magging Novel environment-friendlymaterial material can be obtained, filtrate returns by being dehydrated, being dried at the slurry of de-magging Novel environment-friendlymaterial material
Hydrofluoric acid is prepared to be recycled.
2. the production method of de-magging Novel environment-friendlymaterial material, feature in a kind of Zinc Hydrometallurgy Process according to claim 1
Be: the mass percentage concentration of basic zinc carbonate is 57%.
3. the production method of de-magging Novel environment-friendlymaterial material, feature in a kind of Zinc Hydrometallurgy Process according to claim 1
Be: the temperature of Synthesis is 30-80 DEG C.
4. the production method of de-magging Novel environment-friendlymaterial material, feature in a kind of Zinc Hydrometallurgy Process according to claim 1
Be: the mass percentage concentration of hydrofluoric acid is 12-30%.
5. the production method of de-magging Novel environment-friendlymaterial material, feature in a kind of Zinc Hydrometallurgy Process according to claim 1
It is: performance improving agent A 7L and activator B 3L is added in every cube of basic zinc carbonate.
6. the production method of de-magging Novel environment-friendlymaterial material, feature in a kind of Zinc Hydrometallurgy Process according to claim 1
It is: generated time 2-8h.