CN108691240A - A kind of preparation method of electrostatic prevented corrugated paper plate - Google Patents

A kind of preparation method of electrostatic prevented corrugated paper plate Download PDF

Info

Publication number
CN108691240A
CN108691240A CN201810367748.3A CN201810367748A CN108691240A CN 108691240 A CN108691240 A CN 108691240A CN 201810367748 A CN201810367748 A CN 201810367748A CN 108691240 A CN108691240 A CN 108691240A
Authority
CN
China
Prior art keywords
parts
preparation
water
corrugated paper
paper plate
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201810367748.3A
Other languages
Chinese (zh)
Inventor
冯文田
冯超
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Jurong Xingwu Packaging Co Ltd
Original Assignee
Jurong Xingwu Packaging Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jurong Xingwu Packaging Co Ltd filed Critical Jurong Xingwu Packaging Co Ltd
Priority to CN201810367748.3A priority Critical patent/CN108691240A/en
Publication of CN108691240A publication Critical patent/CN108691240A/en
Pending legal-status Critical Current

Abstract

The invention discloses a kind of preparation methods of electrostatic prevented corrugated paper plate, in corrugated board surface coating substrate glue, after drying again on glue-line be coated with anti-static coatings to get;The substrate glue is made of carragheen, bentonite, cornstarch, citric acid, polylactic acid and water;The anti-static coatings are made of graphene, ethoxylated alkyl ammonium sulfate, epoxy resin, polyacrylamide, sodium alkyl benzene sulfonate, diatomite, antifoaming agent, levelling agent and water.The present invention is first coated with jelly using the method for coating and is coated anti-static coatings using graphene and ethoxylated alkyl ammonium sulfate collaboration as antistatic agent, the suction-operated using jelly enhancing antistatic agent on paper surface, to enhance anti-static electrification.

Description

A kind of preparation method of electrostatic prevented corrugated paper plate
Technical field
The invention belongs to field of packaging material, and in particular to a kind of preparation method of electrostatic prevented corrugated paper plate.
Background technology
Packaging industry is after the pros and cons course that experienced plastics, glass, metal material, and paper products have its wide finally Market is played, corrugated case is a kind of important transportation package holds, its manufacture craft is roughly divided into combined corrugated board, print Brush, in conjunction with etc.;It is made of fluting medium and boxboard respectively.Corrugated board is used as most representative environmentally friendly packing material institute The container of making, it has also become most widely used material in all packagings, it applies to during the entire process of storing and transporting, existing Very important effect is played in the commodity packaging in generation.
Along with the raising of the development and the level of consumption of society, commodity outer packing is more and more taken seriously.Therefore corrugated case As a kind of goods packing container, not only to ensure transporting safely for cargo, but also also need to publicity beautification commodity, promote pin It sells, increases the function of surcharge.In public idea, corrugated case is the production for needing to serve special performance requirement Product, so moisture-proof in needs, the outlet of the extra packages product such as mould proof and antistatic more uses iron, plastics, glass and wood Packing box processed etc., and these packaging for corrugated board, raw material are more expensive and waste is not disposable, the feature of environmental protection compared with Difference;Occupied space is big when storage and transportation, difficult with post-processing;Wooden case outlet need to fumigate.To solve this problem, insider's research With develop functional tile corrugated paper board, and have the packaging of the product applied to all kinds of functional property demands in mind.
Currently, with computer and household electrical appliance fast development and popularizing, the application of integrated circuit is also more and more extensive, close Intensity also goes up very fast, and therefore, the harm in terms of electrostatic is also just more exposed to attention, carries the corrugated board of electrostatic function Also it receives more and more attention and payes attention to.
Invention content
The object of the present invention is to provide a kind of preparation methods of electrostatic prevented corrugated paper plate.
A kind of preparation method of electrostatic prevented corrugated paper plate, in corrugated board surface coating substrate glue, again in glue-line after drying Upper coating anti-static coatings to get;
The substrate glue is made of carragheen, bentonite, cornstarch, citric acid, polylactic acid and water;
The anti-static coatings are by graphene, ethoxylated alkyl ammonium sulfate, epoxy resin, polyacrylamide, benzene sulfonamide Sour sodium, diatomite, antifoaming agent, levelling agent and water are made.
Further, the dosage of each component is in parts by weight in the substrate glue:1-3 parts of carragheen, bentonite 0.5-1 parts, 2-5 parts of cornstarch, 0.2-0.4 parts of citric acid, 0.1-0.5 parts of polylactic acid, 100 parts of water.
Further, the preparation method of the substrate glue, includes the following steps:
Step 1, carragheen, cornstarch and polylactic acid are added to and aqueous solution is made in water;
Step 2, bentonite is dispersed in water and dispersion liquid is made;
Step 3, the aqueous solution of step 1 and the dispersion liquid of step 2 are mixed, citric acid are added, be uniformly mixed to get.
Further, the dosage of each component is in parts by weight in the anti-static coatings:1-3 parts of graphene, ethyoxyl Change 2-5 parts of alkylsurfuric acid ammonium, 20-30 parts of epoxy resin, 2-5 parts of polyacrylamide, 1-3 parts of sodium alkyl benzene sulfonate, diatomite 0.5-1.2 parts, 0.1-0.3 parts of antifoaming agent, 30-50 parts of water.
Further, the preparation method of the anti-static coatings, includes the following steps:
Step 1, epoxy resin, polyacrylamide, diatomite are added in water, is stirred, is uniformly mixed;
Step 2, graphene, ethoxylated alkyl ammonium sulfate and sodium alkyl benzene sulfonate are added under agitation, continues to stir;
Step 3, be added antifoaming agent under agitation, grinding to get.
Further, the coating weight of substrate glue is 4-6g/m2, the coating weight of anti-static coatings is 10-14g/m2
The present invention is first applied using graphene and ethoxylated alkyl ammonium sulfate collaboration as antistatic agent using the method for coating Cloth jelly is coated anti-static coatings, the suction-operated using jelly enhancing antistatic agent on paper surface, to enhance antistatic Effect.
Specific implementation mode
Embodiment 1
A kind of preparation method of electrostatic prevented corrugated paper plate applies on glue-line in corrugated board surface coating substrate glue after drying again Cloth anti-static coatings to get.The coating weight of substrate glue is 4g/m2, the coating weight of anti-static coatings is 10g/m2
The dosage of each component is in parts by weight in the substrate glue:1 part of carragheen, 0.5 part of bentonite, cornstarch 2 parts, 0.2 part of citric acid, 0.1 part of polylactic acid, 100 parts of water.
The dosage of each component is in parts by weight in the anti-static coatings:1 part of graphene, ethoxylated alkyl ammonium sulfate 2 parts, 20 parts of epoxy resin, 2 parts of polyacrylamide, 1 part of sodium alkyl benzene sulfonate, 0.5 part of diatomite, 0.1 part of antifoaming agent, water 30 Part.
Wherein, the preparation method of the substrate glue includes the following steps:
Step 1, carragheen, cornstarch and polylactic acid are added to and aqueous solution is made in water;
Step 2, bentonite is dispersed in water and dispersion liquid is made;
Step 3, the aqueous solution of step 1 and the dispersion liquid of step 2 are mixed, citric acid are added, be uniformly mixed to get.
The preparation method of the anti-static coatings, includes the following steps:
Step 1, epoxy resin, polyacrylamide, diatomite are added in water, is stirred, is uniformly mixed;
Step 2, graphene, ethoxylated alkyl ammonium sulfate and sodium alkyl benzene sulfonate are added under agitation, continues to stir;
Step 3, be added antifoaming agent under agitation, grinding to get.
Gained cardboard is under the conditions of 25 DEG C, relative humidity 65%, bursting strength 1156kPa, and side pressure strength is 398 kPa, is put down Compressive Strength is 475 kPa, and Punctured Strength 4.35J, antistatic intensity is 12.7 × 103Ω.After rubbed 100 times, antistatic Intensity is 13.7 × 103Ω。
Embodiment 2
A kind of preparation method of electrostatic prevented corrugated paper plate applies on glue-line in corrugated board surface coating substrate glue after drying again Cloth anti-static coatings to get.The coating weight of substrate glue is 5g/m2, the coating weight of anti-static coatings is 12g/m2
The dosage of each component is in parts by weight in the substrate glue:2 parts of carragheen, 0.5 part of bentonite, cornstarch 3 parts, 0.3 part of citric acid, 0.3 part of polylactic acid, 100 parts of water.
The dosage of each component is in parts by weight in the anti-static coatings:2 parts of graphene, ethoxylated alkyl ammonium sulfate 4 parts, 23 parts of epoxy resin, 4 parts of polyacrylamide, 2 parts of sodium alkyl benzene sulfonate, 0.7 part of diatomite, 0.2 part of antifoaming agent, water 40 Part.
Wherein, the preparation method of the substrate glue includes the following steps:
Step 1, carragheen, cornstarch and polylactic acid are added to and aqueous solution is made in water;
Step 2, bentonite is dispersed in water and dispersion liquid is made;
Step 3, the aqueous solution of step 1 and the dispersion liquid of step 2 are mixed, citric acid are added, be uniformly mixed to get.
The preparation method of the anti-static coatings, includes the following steps:
Step 1, epoxy resin, polyacrylamide, diatomite are added in water, is stirred, is uniformly mixed;
Step 2, graphene, ethoxylated alkyl ammonium sulfate and sodium alkyl benzene sulfonate are added under agitation, continues to stir;
Step 3, be added antifoaming agent under agitation, grinding to get.
Gained cardboard is under the conditions of 25 DEG C, relative humidity 65%, bursting strength 1217kPa, and side pressure strength is 403 kPa, is put down Compressive Strength is 482 kPa, and Punctured Strength 4.43J, antistatic intensity is 12.6 × 103Ω.After rubbed 100 times, antistatic Intensity is 13.5 × 103Ω。
Embodiment 3
A kind of preparation method of electrostatic prevented corrugated paper plate applies on glue-line in corrugated board surface coating substrate glue after drying again Cloth anti-static coatings to get.The coating weight of substrate glue is 6g/m2, the coating weight of anti-static coatings is 14g/m2
The dosage of each component is in parts by weight in the substrate glue:2 parts of carragheen, 0.7 part of bentonite, cornstarch 4 parts, 0.3 part of citric acid, 0.2 part of polylactic acid, 100 parts of water.
The dosage of each component is in parts by weight in the anti-static coatings:2 parts of graphene, ethoxylated alkyl ammonium sulfate 4 parts, 25 parts of epoxy resin, 4 parts of polyacrylamide, 2 parts of sodium alkyl benzene sulfonate, 0.8 part of diatomite, 0.2 part of antifoaming agent, water 40 Part.
Wherein, the preparation method of the substrate glue includes the following steps:
Step 1, carragheen, cornstarch and polylactic acid are added to and aqueous solution is made in water;
Step 2, bentonite is dispersed in water and dispersion liquid is made;
Step 3, the aqueous solution of step 1 and the dispersion liquid of step 2 are mixed, citric acid are added, be uniformly mixed to get.
The preparation method of the anti-static coatings, includes the following steps:
Step 1, epoxy resin, polyacrylamide, diatomite are added in water, is stirred, is uniformly mixed;
Step 2, graphene, ethoxylated alkyl ammonium sulfate and sodium alkyl benzene sulfonate are added under agitation, continues to stir;
Step 3, be added antifoaming agent under agitation, grinding to get.
Gained cardboard is under the conditions of 25 DEG C, relative humidity 65%, bursting strength 1213kPa, and side pressure strength is 387 kPa, is put down Compressive Strength is 465 kPa, and Punctured Strength 4.29J, antistatic intensity is 12.1 × 103Ω.After rubbed 100 times, antistatic Intensity is 13.4 × 103Ω。

Claims (6)

1. a kind of preparation method of electrostatic prevented corrugated paper plate, it is characterised in that:In corrugated board surface coating substrate glue, after drying Again on glue-line be coated with anti-static coatings to get;
The substrate glue is made of carragheen, bentonite, cornstarch, citric acid, polylactic acid and water;
The anti-static coatings are by graphene, ethoxylated alkyl ammonium sulfate, epoxy resin, polyacrylamide, benzene sulfonamide Sour sodium, diatomite, antifoaming agent, levelling agent and water are made.
2. the preparation method of electrostatic prevented corrugated paper plate according to claim 1, it is characterised in that:Each group in the substrate glue Point dosage be in parts by weight:1-3 parts of carragheen, 0.5-1 parts of bentonite, 2-5 parts of cornstarch, citric acid 0.2- 0.4 part, 0.1-0.5 parts of polylactic acid, 100 parts of water.
3. the preparation method of electrostatic prevented corrugated paper plate according to claim 1, it is characterised in that:The preparation of the substrate glue Method includes the following steps:
Step 1, carragheen, cornstarch and polylactic acid are added to and aqueous solution is made in water;
Step 2, bentonite is dispersed in water and dispersion liquid is made;
Step 3, the aqueous solution of step 1 and the dispersion liquid of step 2 are mixed, citric acid are added, be uniformly mixed to get.
4. the preparation method of electrostatic prevented corrugated paper plate according to claim 1, it is characterised in that:In the anti-static coatings The dosage of each component is in parts by weight:1-3 parts of graphene, 2-5 parts of ethoxylated alkyl ammonium sulfate, 20-30 parts of epoxy resin, 2-5 parts of polyacrylamide, 1-3 parts of sodium alkyl benzene sulfonate, 0.5-1.2 parts of diatomite, 0.1-0.3 parts of antifoaming agent, 30-50 parts of water.
5. the preparation method of electrostatic prevented corrugated paper plate according to claim 1, it is characterised in that:The anti-static coatings Preparation method includes the following steps:
Step 1, epoxy resin, polyacrylamide, diatomite are added in water, is stirred, is uniformly mixed;
Step 2, graphene, ethoxylated alkyl ammonium sulfate and sodium alkyl benzene sulfonate are added under agitation, continues to stir;
Step 3, be added antifoaming agent under agitation, grinding to get.
6. the preparation method of electrostatic prevented corrugated paper plate according to claim 1, it is characterised in that:The coating weight of substrate glue is 4-6g/m2, the coating weight of anti-static coatings is 10-14g/m2
CN201810367748.3A 2018-04-23 2018-04-23 A kind of preparation method of electrostatic prevented corrugated paper plate Pending CN108691240A (en)