CN108611884B - Wool dyeing method capable of improving dye uptake - Google Patents

Wool dyeing method capable of improving dye uptake Download PDF

Info

Publication number
CN108611884B
CN108611884B CN201810256198.8A CN201810256198A CN108611884B CN 108611884 B CN108611884 B CN 108611884B CN 201810256198 A CN201810256198 A CN 201810256198A CN 108611884 B CN108611884 B CN 108611884B
Authority
CN
China
Prior art keywords
wool fabric
temperature
wool
washing
water
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201810256198.8A
Other languages
Chinese (zh)
Other versions
CN108611884A (en
Inventor
卢超标
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Hebei Jinkang Sibo Cashmere Products Co., Ltd
Original Assignee
Hebei Jinkang Sibo Cashmere Products Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Hebei Jinkang Sibo Cashmere Products Co Ltd filed Critical Hebei Jinkang Sibo Cashmere Products Co Ltd
Priority to CN201810256198.8A priority Critical patent/CN108611884B/en
Publication of CN108611884A publication Critical patent/CN108611884A/en
Application granted granted Critical
Publication of CN108611884B publication Critical patent/CN108611884B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a wool dyeing method for improving dye uptake, which comprises the following steps: step one, a pretreatment stage: putting the wool fabric into water; providing a rubber comb tooth which is of a comb-tooth-shaped structure made of rubber and is hollow inside, wherein the rubber comb tooth comprises a transverse connecting part and a plurality of tooth parts arranged on one side of the transverse connecting part side by side, the tail end of each tooth part is provided with an air outlet, and a hot steam supply device is connected to the transverse connecting part through a pipeline; the method comprises the following steps of (1) carding one side surface of a wool fabric by using rubber comb teeth, and pressing the rubber comb teeth on the surface of the wool fabric to enable water absorbed by the wool fabric to seep out of the wool fabric; continuing washing; step two, a dyeing stage: placing in water, adding Natrii sulfas, pH regulator, leveling agent, hydrogen peroxide activator and lubricant, and heating; then heating and adding dye; continuously adding hydrogen peroxide; step three, washing stage. The invention improves the dye uptake and reduces the damage of dyeing treatment to the strength of the dye.

Description

Wool dyeing method capable of improving dye uptake
Technical Field
The invention relates to a dyeing process. More particularly, the present invention relates to a wool dyeing method for increasing dye uptake.
Background
With the social progress and the continuous improvement of living standard, people pay more attention to the personalized demand of wearing clothes, the color system of the fabric for clothes is in a diversified development trend, and the requirements of various large purchasers on the color light of the fabric are higher and higher. As a traditional natural fiber, the wool has the advantages of comfort, warm keeping, difficult deformation and the like after a series of weaving, dyeing and finishing processing, and has high clothing value. The method for improving the yellowish ground color of the wool fabric is bleaching, however, the consumption of hydrogen peroxide for bleaching in the conventional dyeing pretreatment is large, the bleaching temperature is high, the time is long, after the pretreatment, the whiteness of the wool fabric is obviously improved, but after the processes of dyeing, finishing and the like, the physical strength of the finished wool fabric is also greatly reduced, and the damage is serious; however, if the pretreatment is carried out without using hydrogen peroxide for bleaching, the color fastness is affected.
Disclosure of Invention
An object of the present invention is to solve at least the above problems and to provide at least the advantages described later.
To achieve these objects and other advantages in accordance with the present invention, there is provided a wool dyeing method for increasing dye uptake, comprising:
step one, a pretreatment stage:
putting the wool fabric into water, and washing for 10-20 min at the washing temperature of 70-80 ℃;
providing a rubber comb tooth which is of a comb-tooth-shaped structure made of rubber and is hollow inside, wherein the rubber comb tooth comprises a transverse connecting part and a plurality of tooth parts arranged on one side of the transverse connecting part side by side, the tail end of each tooth part is provided with an air outlet hole, and a hot steam supply device is connected to the transverse connecting part through a pipeline; then, the wool fabric is laid flat and unfolded, one side surface of the wool fabric is gradually carded from one end of the wool fabric to the other end of the wool fabric by using rubber comb teeth, after one side surface is carded, the wool fabric is turned over, the other side surface of the wool fabric is carded, and in the carding process, the contact force between the rubber comb teeth and the wool fabric is set as follows: the rubber comb teeth are pressed on the surface of the wool fabric, so that water absorbed by the wool fabric seeps out of the wool fabric, and hot steam with the temperature of 70-80 ℃ is supplied to the transverse connecting part through the hot steam supply device in the carding process; carding each side surface of the wool fabric for 2-4 times;
after finishing carding, adding a detergent into water, then putting the wool fabric into the detergent-containing water, and continuously washing for 20-30 min at the washing temperature of 70-80 ℃;
step two, a dyeing stage:
placing the pretreated wool fabric in water, adding mirabilite, a pH regulator, a leveling agent, a hydrogen peroxide activator and a lubricant, heating to a first temperature platform, wherein the first temperature platform is 30-40 ℃, and preserving heat for 10-20 min under the first temperature platform;
then heating to a second temperature platform, wherein the second temperature platform is 80-90 ℃, adding a dye, and keeping the temperature for 5-10 min under the second temperature platform;
continuously adding hydrogen peroxide, and keeping the temperature for 2-5 min at the second temperature platform;
finally, cooling to normal temperature;
step three, a washing stage:
and (3) placing the wool fabric treated in the dyeing stage in water, heating to a third temperature platform, wherein the third temperature platform is between the first temperature platform and the second temperature platform, and washing for 50-70 min.
Preferably, in the wool dyeing method for improving dye uptake, in the first step, hot steam with the temperature of 70 ℃ is supplied to the transverse connection part through the hot steam supply device during carding.
Preferably, in the wool dyeing method for improving the dye uptake, in the first step, the wool fabric is put into water and washed for 10min at the washing temperature of 70 ℃; after carding, washing is continued for 20min, and the washing temperature is 70 ℃.
Preferably, in the wool dyeing method for improving the dye uptake, in the first step, the interval between two adjacent teeth in the rubber comb teeth is 0.5cm, and the ends of the teeth are hemispheric.
Preferably, in the wool dyeing method for improving the dye uptake, in the first step, the moving speed of the rubber comb teeth is 1cm/s during carding.
Preferably, in the wool dyeing method for improving the dye uptake, in the second step, the first temperature platform is 30 ℃, and the temperature is kept for 10min under the first temperature platform; the second temperature platform is 80 ℃, dye is added, and the temperature is kept for 5min under the second temperature platform; and continuously adding hydrogen peroxide, and keeping the temperature of the second temperature platform for 5 min.
The invention at least comprises the following beneficial effects:
according to the invention, the rubber comb teeth are used for carding the wool fabric, the contact force with the wool fabric is that the moisture absorbed by the wool fabric is enabled to be standard, one side surface of the wool fabric is carded firstly, then the other side surface of the wool fabric is carded, and the wool fibers in the wool fabric are stretched, so that the combination of the dye and the wool fibers can be promoted, the dye uptake is improved, the integral treatment time of the wool fabric is reduced, and the damage of dyeing treatment on the strength of the wool fabric is reduced. Moreover, the rubber comb teeth are soft in texture and cannot damage wool fabric.
Additional advantages, objects, and features of the invention will be set forth in part in the description which follows and in part will become apparent to those having ordinary skill in the art upon examination of the following or may be learned from practice of the invention.
Drawings
Fig. 1 is a schematic structural view of a rubber comb according to an embodiment of the present invention.
Detailed Description
The present invention is further described in detail below with reference to the attached drawings so that those skilled in the art can implement the invention by referring to the description text.
It will be understood that terms such as "having," "including," and "comprising," as used herein, do not preclude the presence or addition of one or more other elements or groups thereof.
The invention provides a wool dyeing method for improving the dye uptake, which comprises the following steps:
step one, a pretreatment stage:
putting the wool fabric into water, and washing for 10-20 min at the washing temperature of 70-80 ℃;
providing a rubber comb tooth 1 which is of a comb-tooth-shaped structure made of rubber and is hollow inside, wherein the rubber comb tooth comprises a transverse connecting part 2 and a plurality of tooth parts 3 arranged on one side of the transverse connecting part side by side, the tail end of each tooth part 3 is provided with an air outlet, and a hot steam supply device 4 is connected to the transverse connecting part through a pipeline; then, the wool fabric is laid flat and unfolded, one side surface of the wool fabric is gradually carded from one end of the wool fabric to the other end of the wool fabric by using rubber comb teeth 1 (as shown in figure 1), after one side surface is carded, the wool fabric is turned over, the other side surface of the wool fabric is carded, and in the carding process, the contact force between the rubber comb teeth and the wool fabric is set as: the rubber comb teeth are pressed on the surface of the wool fabric, so that water absorbed by the wool fabric seeps out of the wool fabric, and hot steam with the temperature of 70-80 ℃ is supplied to the transverse connecting part through the hot steam supply device in the carding process; carding each side surface of the wool fabric for 2-4 times;
after finishing carding, adding a detergent into water, then putting the wool fabric into the detergent-containing water, and continuously washing for 20-30 min at the washing temperature of 70-80 ℃;
step two, a dyeing stage:
placing the pretreated wool fabric in water, adding mirabilite, a pH regulator, a leveling agent, a hydrogen peroxide activator and a lubricant, heating to a first temperature platform, wherein the first temperature platform is 30-40 ℃, and preserving heat for 10-20 min under the first temperature platform;
then heating to a second temperature platform, wherein the second temperature platform is 80-90 ℃, adding a dye, and keeping the temperature for 5-10 min under the second temperature platform;
continuously adding hydrogen peroxide, and keeping the temperature for 2-5 min at the second temperature platform;
finally, cooling to normal temperature;
step three, a washing stage:
and (3) placing the wool fabric treated in the dyeing stage in water, heating to a third temperature platform, wherein the third temperature platform is between the first temperature platform and the second temperature platform, and washing for 50-70 min.
According to the invention, the rubber comb teeth are used for carding the wool fabric, the contact force with the wool fabric is that the moisture absorbed by the wool fabric is enabled to be standard, one side surface of the wool fabric is carded firstly, then the other side surface of the wool fabric is carded, and the wool fibers in the wool fabric are stretched, so that the combination of the dye and the wool fibers can be promoted, the dye uptake is improved, the integral treatment time of the wool fabric is reduced, and the damage of dyeing treatment on the strength of the wool fabric is reduced. Moreover, the rubber comb teeth are soft in texture and cannot damage wool fabric.
In the carding process, hot steam is supplied to the rubber comb teeth through the hot steam supply device, and the hot steam is sprayed out through the air outlet holes of the tooth parts and acts on wool fibers, so that the spreading degree of the wool fibers is improved, and the combination of dye and the wool fibers is promoted.
Meanwhile, the dyeing stage is divided into a plurality of temperature steps, and the wool fabric is treated step by step, so that the dyeing rate of the wool fabric is improved.
And after the third step of washing, the steps of dewatering, drying, softening and shaping and the like are also carried out.
Preferably, in the wool dyeing method for improving dye uptake, in the first step, hot steam with the temperature of 70 ℃ is supplied to the transverse connection part through the hot steam supply device during carding; putting the wool fabric into water, and washing for 10min at the washing temperature of 70 ℃.
Preferably, in the wool dyeing method for improving the dye uptake, in the first step, the wool fabric is put into water and washed for 10min at the washing temperature of 70 ℃; after carding, washing is continued for 20min, and the washing temperature is 70 ℃.
Preferably, in the wool dyeing method for improving the dye uptake, in the first step, the interval between two adjacent teeth in the rubber comb teeth is 0.5cm, and the ends of the teeth are hemispheric.
Preferably, in the wool dyeing method for improving the dye uptake, in the first step, the moving speed of the rubber comb teeth is 1cm/s during carding.
Preferably, in the wool dyeing method for improving the dye uptake, in the second step, the first temperature platform is 30 ℃, and the temperature is kept for 10min under the first temperature platform; the second temperature platform is 80 ℃, dye is added, and the temperature is kept for 5min under the second temperature platform; and continuously adding hydrogen peroxide, and keeping the temperature of the second temperature platform for 5 min.
Example one
Step one, a pretreatment stage:
putting the wool fabric into water, and washing for 10min at the washing temperature of 70 ℃; the mass ratio of water to wool fabric is 3: 1;
providing a rubber comb tooth which is of a comb-tooth-shaped structure made of rubber and is hollow inside, wherein the rubber comb tooth comprises a transverse connecting part and a plurality of tooth parts arranged on one side of the transverse connecting part side by side, the tail end of each tooth part is provided with an air outlet hole, and a hot steam supply device is connected to the transverse connecting part through a pipeline; in the rubber comb teeth, the interval between two adjacent tooth parts is 0.5cm, and the tail ends of the tooth parts are hemispherical; then, the wool fabric is laid flat and unfolded, one side surface of the wool fabric is gradually carded from one end of the wool fabric to the other end of the wool fabric by using rubber comb teeth, after one side surface is carded, the wool fabric is turned over, the other side surface of the wool fabric is carded, and in the carding process, the contact force between the rubber comb teeth and the wool fabric is set as follows: the rubber comb teeth are pressed on the surface of the wool fabric, so that water absorbed by the wool fabric seeps out of the wool fabric, and hot steam with the temperature of 70-80 ℃ is supplied to the transverse connecting part through the hot steam supply device in the carding process; each side surface of the wool fabric is carded for 2 times; the moving speed of the rubber comb teeth is 1 cm/s;
after finishing carding, adding a detergent into water, then putting the wool fabric into the detergent-containing water, and continuously washing for 20min at the washing temperature of 70 ℃; the cleaning agent adopts sima DEPICOL and sodium carbonate, and the mass percentage of the cleaning agent to the wool fabric is 3% and 1% respectively;
step two, a dyeing stage:
putting the pretreated wool fabric into water, adding mirabilite, a pH regulator, a leveling agent, a hydrogen peroxide activator and a lubricant, heating to a first temperature platform, wherein the first temperature platform is 30 ℃, and preserving heat for 10min under the first temperature platform; wherein the pH regulator is acetic acid and sodium acetate, the leveling agent is Albizzia SET, the hydrogen peroxide activator is PO brightening agent, and the lubricant is BAIBAO C; the weight percentages of the mirabilite, the pH regulator, the leveling agent, the hydrogen peroxide activator and the lubricant to the wool fabric are respectively 3%, 1%, 7%, 3% and 3.5%; the mass ratio of water to wool fabric is 3: 1;
then heating to a second temperature platform, wherein the second temperature platform is 80 ℃, adding a dye, and keeping the temperature for 5min under the second temperature platform; the dye is an acid dye in an Elille series, and the mass ratio of the dye to the wool fabric is 2.8%;
continuously adding hydrogen peroxide, and keeping the temperature for 2min at the second temperature platform; the mass percentage of the hydrogen peroxide and the wool fabric is 8%;
finally, cooling to normal temperature;
step three, a washing stage:
and (3) placing the wool fabric treated in the dyeing stage in water, heating to a third temperature platform, wherein the third temperature platform is between the first temperature platform and the second temperature platform, the temperature is 50 ℃, and washing for 50 min.
Example two
A method of dyeing wool to increase dye uptake comprising:
step one, a pretreatment stage:
putting the wool fabric into water, and washing for 20min at the washing temperature of 80 ℃; the mass ratio of water to wool fabric is 3: 1;
providing a rubber comb tooth which is of a comb-tooth-shaped structure made of rubber and is hollow inside, wherein the rubber comb tooth comprises a transverse connecting part and a plurality of tooth parts arranged on one side of the transverse connecting part side by side, the tail end of each tooth part is provided with an air outlet hole, and a hot steam supply device is connected to the transverse connecting part through a pipeline; in the rubber comb teeth, the interval between two adjacent tooth parts is 0.5cm, and the tail ends of the tooth parts are hemispherical; then, the wool fabric is laid flat and unfolded, one side surface of the wool fabric is gradually carded from one end of the wool fabric to the other end of the wool fabric by using rubber comb teeth, after one side surface is carded, the wool fabric is turned over, the other side surface of the wool fabric is carded, and in the carding process, the contact force between the rubber comb teeth and the wool fabric is set as follows: the rubber comb teeth are pressed against the surface of the wool fabric, so that water absorbed by the wool fabric seeps out from the inside of the wool fabric, and hot steam with the temperature of 70 ℃ is supplied to the transverse connecting part through the hot steam supply device during carding; each side surface of the wool fabric is carded for 4 times; the moving speed of the rubber comb teeth is 1 cm/s;
after finishing carding, adding a detergent into water, then putting the wool fabric into the detergent-containing water, and continuously washing for 30min at the washing temperature of 80 ℃; the cleaning agent adopts sima DEPICOL and sodium carbonate, and the mass percentage of the cleaning agent to the wool fabric is 3% and 1% respectively;
step two, a dyeing stage:
putting the pretreated wool fabric into water, adding mirabilite, a pH regulator, a leveling agent, a hydrogen peroxide activator and a lubricant, heating to a first temperature platform, wherein the first temperature platform is 40 ℃, and keeping the temperature for 20min under the first temperature platform; wherein the pH regulator is acetic acid and sodium acetate, the leveling agent is Albizzia SET, the hydrogen peroxide activator is PO brightening agent, and the lubricant is BAIBAO C; the weight percentages of the mirabilite, the pH regulator, the leveling agent, the hydrogen peroxide activator and the lubricant to the wool fabric are respectively 3%, 1%, 7%, 3% and 3.5%; the mass ratio of water to wool fabric is 3: 1;
then heating to a second temperature platform, wherein the second temperature platform is 90 ℃, adding a dye, and keeping the temperature for 10min under the second temperature platform; the dye is an acid dye of an Elille series, and the mass ratio of the dye to the wool fabric is 2.8%:
continuously adding hydrogen peroxide, and keeping the temperature of the second temperature platform for 5 min; the mass percentage of the hydrogen peroxide and the wool fabric is 8%;
finally, cooling to normal temperature;
step three, a washing stage:
and (3) placing the wool fabric treated in the dyeing stage in water, heating to a third temperature platform, wherein the third temperature platform is between the first temperature platform and the second temperature platform, the temperature is 50 ℃, and washing for 70 min.
EXAMPLE III
A method of dyeing wool to increase dye uptake comprising:
step one, a pretreatment stage:
putting the wool fabric into water, and washing for 20min at the washing temperature of 70 ℃; the mass ratio of water to wool fabric is 3: 1;
providing a rubber comb tooth which is of a comb-tooth-shaped structure made of rubber and is hollow inside, wherein the rubber comb tooth comprises a transverse connecting part and a plurality of tooth parts arranged on one side of the transverse connecting part side by side, the tail end of each tooth part is provided with an air outlet hole, and a hot steam supply device is connected to the transverse connecting part through a pipeline; in the rubber comb teeth, the interval between two adjacent tooth parts is 0.5cm, and the tail ends of the tooth parts are hemispherical; then, the wool fabric is laid flat and unfolded, one side surface of the wool fabric is gradually carded from one end of the wool fabric to the other end of the wool fabric by using rubber comb teeth, after one side surface is carded, the wool fabric is turned over, the other side surface of the wool fabric is carded, and in the carding process, the contact force between the rubber comb teeth and the wool fabric is set as follows: the rubber comb teeth are pressed against the surface of the wool fabric, so that water absorbed by the wool fabric seeps out from the inside of the wool fabric, and hot steam with the temperature of 80 ℃ is supplied to the transverse connecting part through the hot steam supply device during carding; each side surface of the wool fabric is carded for 2 times; the moving speed of the rubber comb teeth is 1 cm/s;
after finishing carding, adding a detergent into water, then putting the wool fabric into the detergent-containing water, and continuously washing for 20min at the washing temperature of 70 ℃; the cleaning agent adopts sima DEPICOL and sodium carbonate, and the mass percentage of the cleaning agent to the wool fabric is 3% and 1% respectively;
step two, a dyeing stage:
putting the pretreated wool fabric into water, adding mirabilite, a pH regulator, a leveling agent, a hydrogen peroxide activator and a lubricant, heating to a first temperature platform, wherein the first temperature platform is 35 ℃, and preserving heat for 10min under the first temperature platform; wherein the pH regulator is acetic acid and sodium acetate, the leveling agent is Albizzia SET, the hydrogen peroxide activator is PO brightening agent, and the lubricant is BAIBAO C; the weight percentages of the mirabilite, the pH regulator, the leveling agent, the hydrogen peroxide activator and the lubricant to the wool fabric are respectively 3%, 1%, 7%, 3% and 3.5%; the mass ratio of water to wool fabric is 3: 1;
then heating to a second temperature platform, wherein the second temperature platform is 90 ℃, adding a dye, and keeping the temperature for 10min under the second temperature platform; the dye is an acid dye of an Elille series, and the mass ratio of the dye to the wool fabric is 2.8%:
continuously adding hydrogen peroxide, and keeping the temperature of the second temperature platform for 5 min; the mass percentage of the hydrogen peroxide and the wool fabric is 8%;
finally, cooling to normal temperature;
step three, a washing stage:
and (3) placing the wool fabric treated in the dyeing stage in water, heating to a third temperature platform, wherein the third temperature platform is between the first temperature platform and the second temperature platform, the temperature is 50 ℃, and washing for 70 min.
Example four
A method of dyeing wool to increase dye uptake comprising:
step one, a pretreatment stage:
putting the wool fabric into water, and washing for 20min at the washing temperature of 75 ℃; the mass ratio of water to wool fabric is 3: 1;
providing a rubber comb tooth which is of a comb-tooth-shaped structure made of rubber and is hollow inside, wherein the rubber comb tooth comprises a transverse connecting part and a plurality of tooth parts arranged on one side of the transverse connecting part side by side, the tail end of each tooth part is provided with an air outlet hole, and a hot steam supply device is connected to the transverse connecting part through a pipeline; in the rubber comb teeth, the interval between two adjacent tooth parts is 0.5cm, and the tail ends of the tooth parts are hemispherical; then, the wool fabric is laid flat and unfolded, one side surface of the wool fabric is gradually carded from one end of the wool fabric to the other end of the wool fabric by using rubber comb teeth, after one side surface is carded, the wool fabric is turned over, the other side surface of the wool fabric is carded, and in the carding process, the contact force between the rubber comb teeth and the wool fabric is set as follows: the rubber comb teeth are pressed against the surface of the wool fabric, so that water absorbed by the wool fabric seeps out from the inside of the wool fabric, and hot steam with the temperature of 80 ℃ is supplied to the transverse connecting part through the hot steam supply device during carding; each side surface of the wool fabric is carded for 2 times; the moving speed of the rubber comb teeth is 1 cm/s;
after finishing carding, adding a detergent into water, then putting the wool fabric into the detergent-containing water, and continuously washing for 20min at the washing temperature of 75 ℃; the cleaning agent adopts sima DEPICOL and sodium carbonate, and the mass percentage of the cleaning agent to the wool fabric is 3% and 1% respectively;
step two, a dyeing stage:
putting the pretreated wool fabric into water, adding mirabilite, a pH regulator, a leveling agent, a hydrogen peroxide activator and a lubricant, heating to a first temperature platform, wherein the first temperature platform is 40 ℃, and keeping the temperature for 20min under the first temperature platform; wherein the pH regulator is acetic acid and sodium acetate, the leveling agent is Albizzia SET, the hydrogen peroxide activator is PO brightening agent, and the lubricant is BAIBAO C; the weight percentages of the mirabilite, the pH regulator, the leveling agent, the hydrogen peroxide activator and the lubricant to the wool fabric are respectively 3%, 1%, 7%, 3% and 3.5%; the mass ratio of water to wool fabric is 3: 1;
then heating to a second temperature platform, wherein the second temperature platform is 90 ℃, adding a dye, and keeping the temperature for 10min under the second temperature platform; the dye is an acid dye of an Elille series, and the mass ratio of the dye to the wool fabric is 2.8%:
continuously adding hydrogen peroxide, and keeping the temperature of the second temperature platform for 4 min; the mass percentage of the hydrogen peroxide and the wool fabric is 8%;
finally, cooling to normal temperature;
step three, a washing stage:
and (3) placing the wool fabric treated in the dyeing stage in water, heating to a third temperature platform, wherein the third temperature platform is between the first temperature platform and the second temperature platform, the temperature is 50 ℃, and washing for 55 min.
EXAMPLE five
A method of dyeing wool to increase dye uptake comprising:
step one, a pretreatment stage:
putting the wool fabric into water, and washing for 14min at the washing temperature of 70 ℃; the mass ratio of water to wool fabric is 3: 1;
providing a rubber comb tooth which is of a comb-tooth-shaped structure made of rubber and is hollow inside, wherein the rubber comb tooth comprises a transverse connecting part and a plurality of tooth parts arranged on one side of the transverse connecting part side by side, the tail end of each tooth part is provided with an air outlet hole, and a hot steam supply device is connected to the transverse connecting part through a pipeline; in the rubber comb teeth, the interval between two adjacent tooth parts is 0.5cm, and the tail ends of the tooth parts are hemispherical; then, the wool fabric is laid flat and unfolded, one side surface of the wool fabric is gradually carded from one end of the wool fabric to the other end of the wool fabric by using rubber comb teeth, after one side surface is carded, the wool fabric is turned over, the other side surface of the wool fabric is carded, and in the carding process, the contact force between the rubber comb teeth and the wool fabric is set as follows: the rubber comb teeth are pressed against the surface of the wool fabric, so that water absorbed by the wool fabric seeps out from the inside of the wool fabric, and hot steam with the temperature of 80 ℃ is supplied to the transverse connecting part through the hot steam supply device during carding; each side surface of the wool fabric is carded for 4 times; the moving speed of the rubber comb teeth is 1 cm/s;
after finishing carding, adding a detergent into water, then putting the wool fabric into the detergent-containing water, and continuously washing for 25min at the washing temperature of 70 ℃; the cleaning agent adopts sima DEPICOL and sodium carbonate, and the mass percentage of the cleaning agent to the wool fabric is 3% and 1% respectively;
step two, a dyeing stage:
putting the pretreated wool fabric into water, adding mirabilite, a pH regulator, a leveling agent, a hydrogen peroxide activator and a lubricant, heating to a first temperature platform, wherein the first temperature platform is 30 ℃, and keeping the temperature for 15min under the first temperature platform; wherein the pH regulator is acetic acid and sodium acetate, the leveling agent is Albizzia SET, the hydrogen peroxide activator is PO brightening agent, and the lubricant is BAIBAO C; the weight percentages of the mirabilite, the pH regulator, the leveling agent, the hydrogen peroxide activator and the lubricant to the wool fabric are respectively 3%, 1%, 7%, 3% and 3.5%; the mass ratio of water to wool fabric is 3: 1;
then heating to a second temperature platform, wherein the second temperature platform is 80 ℃, adding a dye, and keeping the temperature for 10min under the second temperature platform; the dye is an acid dye of an Elille series, and the mass ratio of the dye to the wool fabric is 2.8%:
continuously adding hydrogen peroxide, and keeping the temperature for 2min at the second temperature platform; the mass percentage of the hydrogen peroxide and the wool fabric is 8%;
finally, cooling to normal temperature;
step three, a washing stage:
and (3) placing the wool fabric treated in the dyeing stage in water, heating to a third temperature platform, wherein the third temperature platform is between the first temperature platform and the second temperature platform, the temperature is 50 ℃, and washing for 50 min.
EXAMPLE six
A method of dyeing wool to increase dye uptake comprising:
step one, a pretreatment stage:
putting the wool fabric into water, and washing for 10min at the washing temperature of 80 ℃; the mass ratio of water to wool fabric is 3: 1;
providing a rubber comb tooth which is of a comb-tooth-shaped structure made of rubber and is hollow inside, wherein the rubber comb tooth comprises a transverse connecting part and a plurality of tooth parts arranged on one side of the transverse connecting part side by side, the tail end of each tooth part is provided with an air outlet hole, and a hot steam supply device is connected to the transverse connecting part through a pipeline; in the rubber comb teeth, the interval between two adjacent tooth parts is 0.5cm, and the tail ends of the tooth parts are hemispherical; then, the wool fabric is laid flat and unfolded, one side surface of the wool fabric is gradually carded from one end of the wool fabric to the other end of the wool fabric by using rubber comb teeth, after one side surface is carded, the wool fabric is turned over, the other side surface of the wool fabric is carded, and in the carding process, the contact force between the rubber comb teeth and the wool fabric is set as follows: the rubber comb teeth are pressed against the surface of the wool fabric, so that water absorbed by the wool fabric seeps out from the inside of the wool fabric, and hot steam with the temperature of 70 ℃ is supplied to the transverse connecting part through the hot steam supply device during carding; each side surface of the wool fabric is carded for 3 times; the moving speed of the rubber comb teeth is 1 cm/s;
after finishing carding, adding a detergent into water, then putting the wool fabric into the detergent-containing water, and continuously washing for 20min at the washing temperature of 70 ℃; the cleaning agent adopts sima DEPICOL and sodium carbonate, and the mass percentage of the cleaning agent to the wool fabric is 3% and 1% respectively;
step two, a dyeing stage:
putting the pretreated wool fabric into water, adding mirabilite, a pH regulator, a leveling agent, a hydrogen peroxide activator and a lubricant, heating to a first temperature platform, wherein the first temperature platform is 35 ℃, and preserving heat for 10min under the first temperature platform; wherein the pH regulator is acetic acid and sodium acetate, the leveling agent is Albizzia SET, the hydrogen peroxide activator is PO brightening agent, and the lubricant is BAIBAO C; the weight percentages of the mirabilite, the pH regulator, the leveling agent, the hydrogen peroxide activator and the lubricant to the wool fabric are respectively 3%, 1%, 7%, 3% and 3.5%; the mass ratio of water to wool fabric is 3: 1;
then heating to a second temperature platform, wherein the second temperature platform is 85 ℃, adding a dye, and keeping the temperature for 6min under the second temperature platform; the dye is an acid dye in an Elille series, and the mass ratio of the dye to the wool fabric is 2.8%;
continuously adding hydrogen peroxide, and keeping the temperature for 2min at the second temperature platform; the mass percentage of the hydrogen peroxide and the wool fabric is 8%;
finally, cooling to normal temperature;
step three, a washing stage:
and (3) placing the wool fabric treated in the dyeing stage in water, heating to a third temperature platform, wherein the third temperature platform is between the first temperature platform and the second temperature platform, the temperature is 50 ℃, and washing for 55 min.
EXAMPLE seven
A method of dyeing wool to increase dye uptake comprising:
step one, a pretreatment stage:
putting the wool fabric into water, and washing for 15min at the washing temperature of 75 ℃; the mass ratio of water to wool fabric is 3: 1;
providing a rubber comb tooth which is of a comb-tooth-shaped structure made of rubber and is hollow inside, wherein the rubber comb tooth comprises a transverse connecting part and a plurality of tooth parts arranged on one side of the transverse connecting part side by side, the tail end of each tooth part is provided with an air outlet hole, and a hot steam supply device is connected to the transverse connecting part through a pipeline; in the rubber comb teeth, the interval between two adjacent tooth parts is 0.5cm, and the tail ends of the tooth parts are hemispherical; then, the wool fabric is laid flat and unfolded, one side surface of the wool fabric is gradually carded from one end of the wool fabric to the other end of the wool fabric by using rubber comb teeth, after one side surface is carded, the wool fabric is turned over, the other side surface of the wool fabric is carded, and in the carding process, the contact force between the rubber comb teeth and the wool fabric is set as follows: the rubber comb teeth are pressed against the surface of the wool fabric, so that water absorbed by the wool fabric seeps out from the inside of the wool fabric, and hot steam with the temperature of 75 ℃ is supplied to the transverse connecting part through the hot steam supply device during carding; each side surface of the wool fabric is carded for 2 times; the moving speed of the rubber comb teeth is 1 cm/s;
after finishing carding, adding a detergent into water, then putting the wool fabric into the detergent-containing water, and continuously washing for 22min at the washing temperature of 75 ℃; the cleaning agent adopts sima DEPICOL and sodium carbonate, and the mass percentage of the cleaning agent to the wool fabric is 3% and 1% respectively;
step two, a dyeing stage:
putting the pretreated wool fabric into water, adding mirabilite, a pH regulator, a leveling agent, a hydrogen peroxide activator and a lubricant, heating to a first temperature platform, wherein the first temperature platform is 34 ℃, and keeping the temperature for 15min under the first temperature platform; wherein the pH regulator is acetic acid and sodium acetate, the leveling agent is Albizzia SET, the hydrogen peroxide activator is PO brightening agent, and the lubricant is BAIBAO C; the weight percentages of the mirabilite, the pH regulator, the leveling agent, the hydrogen peroxide activator and the lubricant to the wool fabric are respectively 3%, 1%, 7%, 3% and 3.5%; the mass ratio of water to wool fabric is 3: 1;
then heating to a second temperature platform, wherein the second temperature platform is 84 ℃, adding a dye, and keeping the temperature for 6min under the second temperature platform; the dye is an acid dye in an Elille series, and the mass ratio of the dye to the wool fabric is 2.8%;
continuously adding hydrogen peroxide, and keeping the temperature for 2min at the second temperature platform; the mass percentage of the hydrogen peroxide and the wool fabric is 8%;
finally, cooling to normal temperature;
step three, a washing stage:
and (3) placing the wool fabric treated in the dyeing stage in water, heating to a third temperature platform, wherein the third temperature platform is between the first temperature platform and the second temperature platform, the temperature is 50 ℃, and washing for 50 min.
Example eight
A method of dyeing wool to increase dye uptake comprising:
step one, a pretreatment stage:
putting the wool fabric into water, and washing for 10min at the washing temperature of 70 ℃; the mass ratio of water to wool fabric is 3: 1;
providing a rubber comb tooth which is of a comb-tooth-shaped structure made of rubber and is hollow inside, wherein the rubber comb tooth comprises a transverse connecting part and a plurality of tooth parts arranged on one side of the transverse connecting part side by side, the tail end of each tooth part is provided with an air outlet hole, and a hot steam supply device is connected to the transverse connecting part through a pipeline; in the rubber comb teeth, the interval between two adjacent tooth parts is 0.5cm, and the tail ends of the tooth parts are hemispherical; then, the wool fabric is laid flat and unfolded, one side surface of the wool fabric is gradually carded from one end of the wool fabric to the other end of the wool fabric by using rubber comb teeth, after one side surface is carded, the wool fabric is turned over, the other side surface of the wool fabric is carded, and in the carding process, the contact force between the rubber comb teeth and the wool fabric is set as follows: the rubber comb teeth are pressed against the surface of the wool fabric, so that water absorbed by the wool fabric seeps out from the inside of the wool fabric, and hot steam with the temperature of 80 ℃ is supplied to the transverse connecting part through the hot steam supply device during carding; each side surface of the wool fabric is carded for 4 times; the moving speed of the rubber comb teeth is 1 cm/s;
after finishing carding, adding a detergent into water, then putting the wool fabric into the detergent-containing water, and continuously washing for 20min at the washing temperature of 70 ℃; the cleaning agent adopts sima DEPICOL and sodium carbonate, and the mass percentage of the cleaning agent to the wool fabric is 3% and 1% respectively;
step two, a dyeing stage:
putting the pretreated wool fabric into water, adding mirabilite, a pH regulator, a leveling agent, a hydrogen peroxide activator and a lubricant, heating to a first temperature platform, wherein the first temperature platform is 36 ℃, and preserving heat for 16min under the first temperature platform; wherein the pH regulator is acetic acid and sodium acetate, the leveling agent is Albizzia SET, the hydrogen peroxide activator is PO brightening agent, and the lubricant is BAIBAO C; the weight percentages of the mirabilite, the pH regulator, the leveling agent, the hydrogen peroxide activator and the lubricant to the wool fabric are respectively 3%, 1%, 7%, 3% and 3.5%; the mass ratio of water to wool fabric is 3: 1;
then heating to a second temperature platform, wherein the second temperature platform is 84 ℃, adding a dye, and keeping the temperature for 7min under the second temperature platform; the dye is an acid dye in an Elille series, and the mass ratio of the dye to the wool fabric is 2.8%;
continuously adding hydrogen peroxide, and keeping the temperature for 2min at the second temperature platform; the mass percentage of the hydrogen peroxide and the wool fabric is 8%;
finally, cooling to normal temperature;
step three, a washing stage:
and (3) placing the wool fabric treated in the dyeing stage in water, heating to a third temperature platform, wherein the third temperature platform is between the first temperature platform and the second temperature platform, the temperature is 50 ℃, and washing for 50 min.
Example nine
A method of dyeing wool to increase dye uptake comprising:
step one, a pretreatment stage:
putting the wool fabric into water, and washing for 12min at the washing temperature of 72 ℃; the mass ratio of water to wool fabric is 3: 1;
providing a rubber comb tooth which is of a comb-tooth-shaped structure made of rubber and is hollow inside, wherein the rubber comb tooth comprises a transverse connecting part and a plurality of tooth parts arranged on one side of the transverse connecting part side by side, the tail end of each tooth part is provided with an air outlet hole, and a hot steam supply device is connected to the transverse connecting part through a pipeline; in the rubber comb teeth, the interval between two adjacent tooth parts is 0.5cm, and the tail ends of the tooth parts are hemispherical; then, the wool fabric is laid flat and unfolded, one side surface of the wool fabric is gradually carded from one end of the wool fabric to the other end of the wool fabric by using rubber comb teeth, after one side surface is carded, the wool fabric is turned over, the other side surface of the wool fabric is carded, and in the carding process, the contact force between the rubber comb teeth and the wool fabric is set as follows: the rubber comb teeth are pressed against the surface of the wool fabric, so that water absorbed by the wool fabric seeps out from the inside of the wool fabric, and hot steam with the temperature of 75 ℃ is supplied to the transverse connecting part through the hot steam supply device during carding; each side surface of the wool fabric is carded for 2 times; the moving speed of the rubber comb teeth is 1 cm/s;
after finishing carding, adding a detergent into water, then putting the wool fabric into the detergent-containing water, and continuously washing for 20min at the washing temperature of 70 ℃; the cleaning agent adopts sima DEPICOL and sodium carbonate, and the mass percentage of the cleaning agent to the wool fabric is 3% and 1% respectively;
step two, a dyeing stage:
putting the pretreated wool fabric into water, adding mirabilite, a pH regulator, a leveling agent, a hydrogen peroxide activator and a lubricant, heating to a first temperature platform, wherein the first temperature platform is 35 ℃, and keeping the temperature for 15min under the first temperature platform; wherein the pH regulator is acetic acid and sodium acetate, the leveling agent is Albizzia SET, the hydrogen peroxide activator is PO brightening agent, and the lubricant is BAIBAO C; the weight percentages of the mirabilite, the pH regulator, the leveling agent, the hydrogen peroxide activator and the lubricant to the wool fabric are respectively 3%, 1%, 7%, 3% and 3.5%; the mass ratio of water to wool fabric is 3: 1;
then heating to a second temperature platform, wherein the second temperature platform is 86 ℃, adding a dye, and keeping the temperature for 10min under the second temperature platform; the dye is an acid dye in an Elille series, and the mass ratio of the dye to the wool fabric is 2.8%;
continuously adding hydrogen peroxide, and keeping the temperature of the second temperature platform for 5 min; the mass percentage of the hydrogen peroxide and the wool fabric is 8%;
finally, cooling to normal temperature;
step three, a washing stage:
and (3) placing the wool fabric treated in the dyeing stage in water, heating to a third temperature platform, wherein the third temperature platform is between the first temperature platform and the second temperature platform, the temperature is 50 ℃, and washing for 60 min.
Example ten
A method of dyeing wool to increase dye uptake comprising:
step one, a pretreatment stage:
putting the wool fabric into water, and washing for 15min at the washing temperature of 70 ℃; the mass ratio of water to wool fabric is 3: 1;
providing a rubber comb tooth which is of a comb-tooth-shaped structure made of rubber and is hollow inside, wherein the rubber comb tooth comprises a transverse connecting part and a plurality of tooth parts arranged on one side of the transverse connecting part side by side, the tail end of each tooth part is provided with an air outlet hole, and a hot steam supply device is connected to the transverse connecting part through a pipeline; in the rubber comb teeth, the interval between two adjacent tooth parts is 0.5cm, and the tail ends of the tooth parts are hemispherical; then, the wool fabric is laid flat and unfolded, one side surface of the wool fabric is gradually carded from one end of the wool fabric to the other end of the wool fabric by using rubber comb teeth, after one side surface is carded, the wool fabric is turned over, the other side surface of the wool fabric is carded, and in the carding process, the contact force between the rubber comb teeth and the wool fabric is set as follows: the rubber comb teeth are pressed against the surface of the wool fabric, so that water absorbed by the wool fabric seeps out from the inside of the wool fabric, and hot steam with the temperature of 70 ℃ is supplied to the transverse connecting part through the hot steam supply device during carding; each side surface of the wool fabric is carded for 2 times; the moving speed of the rubber comb teeth is 1 cm/s;
after finishing carding, adding a detergent into water, then putting the wool fabric into the detergent-containing water, and continuously washing for 2min at the washing temperature of 70 ℃; the cleaning agent adopts sima DEPICOL and sodium carbonate, and the mass percentage of the cleaning agent to the wool fabric is 3% and 1% respectively;
step two, a dyeing stage:
putting the pretreated wool fabric into water, adding mirabilite, a pH regulator, a leveling agent, a hydrogen peroxide activator and a lubricant, heating to a first temperature platform, wherein the first temperature platform is 32 ℃, and keeping the temperature for 12min under the first temperature platform; wherein the pH regulator is acetic acid and sodium acetate, the leveling agent is Albizzia SET, the hydrogen peroxide activator is PO brightening agent, and the lubricant is BAIBAO C; the weight percentages of the mirabilite, the pH regulator, the leveling agent, the hydrogen peroxide activator and the lubricant to the wool fabric are respectively 3%, 1%, 7%, 3% and 3.5%; the mass ratio of water to wool fabric is 3: 1;
then heating to a second temperature platform, wherein the second temperature platform is 84 ℃, adding a dye, and keeping the temperature for 6min under the second temperature platform; the dye is an acid dye in an Elille series, and the mass ratio of the dye to the wool fabric is 2.8%;
continuously adding hydrogen peroxide, and keeping the temperature of the second temperature platform for 5 min; the mass percentage of the hydrogen peroxide and the wool fabric is 8%;
finally, cooling to normal temperature;
step three, a washing stage:
and (3) putting the wool fabric treated in the dyeing stage into water, heating to a third temperature platform, wherein the third temperature platform is between the first temperature platform and the second temperature platform, the temperature is 50 ℃, and washing for 56 min.
Comparative example
The prior art is adopted to dye the wool fabric. The wool fabric is placed in a washing solution for washing, and then placed in a dyeing solution containing a pH regulator, mirabilite and a dye for dyeing.
The indices of the wool fabrics of examples one to ten and the comparative example are shown in table 1. And detecting the dye uptake of the wool fabric by adopting spectrophotometry. And (3) extracting wool fibers from 10 wool fabrics, detecting the strength by adopting an electronic single fiber strength tester, and taking an average value. As can be seen from Table 1, the invention can improve the dye uptake and the fiber strength of the wool fabric.
TABLE 1
Figure BDA0001609028750000181
Figure BDA0001609028750000191
While embodiments of the invention have been disclosed above, it is not intended to be limited to the uses set forth in the specification and examples. It can be applied to all kinds of fields suitable for the present invention. Additional modifications will readily occur to those skilled in the art. It is therefore intended that the invention not be limited to the exact details and illustrations described and illustrated herein, but fall within the scope of the appended claims and equivalents thereof.

Claims (4)

1. The wool dyeing method for improving the dye uptake is characterized by comprising the following steps:
step one, a pretreatment stage:
putting the wool fabric into water, and washing for 10-20 min at the washing temperature of 70-80 ℃;
providing a rubber comb tooth which is of a comb-tooth-shaped structure made of rubber and is hollow inside, wherein the rubber comb tooth comprises a transverse connecting part and a plurality of tooth parts arranged on one side of the transverse connecting part side by side, the tail end of each tooth part is provided with an air outlet hole, and a hot steam supply device is connected to the transverse connecting part through a pipeline; then, the wool fabric is laid flat and unfolded, one side surface of the wool fabric is gradually carded from one end of the wool fabric to the other end of the wool fabric by using rubber comb teeth, after one side surface is carded, the wool fabric is turned over, the other side surface of the wool fabric is carded, and in the carding process, the contact force between the rubber comb teeth and the wool fabric is set as follows: the rubber comb teeth are pressed on the surface of the wool fabric, so that water absorbed by the wool fabric seeps out of the wool fabric, and hot steam with the temperature of 70-80 ℃ is supplied to the transverse connecting part through the hot steam supply device in the carding process; carding each side surface of the wool fabric for 2-4 times; in the rubber comb teeth, the interval between two adjacent tooth parts is 0.5cm, and the tail ends of the tooth parts are hemispherical; in the carding process, the moving speed of the rubber comb teeth is 1 cm/s;
after finishing carding, adding a detergent into water, then putting the wool fabric into the detergent-containing water, and continuously washing for 20-30 min at the washing temperature of 70-80 ℃;
step two, a dyeing stage:
placing the pretreated wool fabric in water, adding mirabilite, a pH regulator, a leveling agent, a hydrogen peroxide activator and a lubricant, heating to a first temperature platform, wherein the first temperature platform is 30-40 ℃, and preserving heat for 10-20 min under the first temperature platform;
then heating to a second temperature platform, wherein the second temperature platform is 80-90 ℃, adding a dye, and keeping the temperature for 5-10 min under the second temperature platform;
continuously adding hydrogen peroxide, and keeping the temperature for 2-5 min at the second temperature platform;
finally, cooling to normal temperature;
step three, a washing stage:
and (3) placing the wool fabric treated in the dyeing stage in water, heating to a third temperature platform, wherein the third temperature platform is between the first temperature platform and the second temperature platform, and washing for 50-70 min.
2. A wool dyeing method with improved dye uptake according to claim 1, characterized in that in step one, hot steam with a temperature of 70 ℃ is supplied to the transverse connection by the hot steam supply device during carding.
3. A wool dyeing method for improving dye uptake according to claim 2, characterized in that in the first step, the wool fabric is put into water and washed for 10min at the temperature of 70 ℃; after carding, washing is continued for 20min, and the washing temperature is 70 ℃.
4. A method for dyeing wool to increase the dye uptake according to claim 1, wherein in step two, the first temperature plateau is 30 ℃ and the temperature is maintained at the first temperature plateau for 10 min; the second temperature platform is 80 ℃, dye is added, and the temperature is kept for 5min under the second temperature platform; and continuously adding hydrogen peroxide, and keeping the temperature of the second temperature platform for 5 min.
CN201810256198.8A 2018-03-27 2018-03-27 Wool dyeing method capable of improving dye uptake Active CN108611884B (en)