CN107190380A - Containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton - Google Patents

Containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton Download PDF

Info

Publication number
CN107190380A
CN107190380A CN201710431894.3A CN201710431894A CN107190380A CN 107190380 A CN107190380 A CN 107190380A CN 201710431894 A CN201710431894 A CN 201710431894A CN 107190380 A CN107190380 A CN 107190380A
Authority
CN
China
Prior art keywords
cotton
hemp
spinning process
revs
hemps
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201710431894.3A
Other languages
Chinese (zh)
Other versions
CN107190380B (en
Inventor
朱华
沈春明
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
ZHEJIANG LONGYUAN TEXTILE Co.,Ltd.
Original Assignee
Jiaxing Longyuan Trading Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jiaxing Longyuan Trading Co Ltd filed Critical Jiaxing Longyuan Trading Co Ltd
Priority to CN201710431894.3A priority Critical patent/CN107190380B/en
Publication of CN107190380A publication Critical patent/CN107190380A/en
Application granted granted Critical
Publication of CN107190380B publication Critical patent/CN107190380B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

Containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton, belong to textile technology field.It includes taking hemp and cotton fiber material, hemp is carried out to wet process, again in the public fixed Eight-Diagram of 55/ cotton of ratio hemp 45 arrangement of weighing that gets damp again, 528 grams m laps are made through cotton cleaning process, then through cotton carding, it is pre- simultaneously, in rolls, combing, end simultaneously, rove, spun yarn, winding procedure produce the scribbled of the fiber containing hemp/cotton.Instant invention overcomes the spinning process that hemp is not suitable with cotton spinning process, substantially increase content ratio of the hemp in mixed yarn, making the fabric of hemp/cotton blended yarn, not only the moisture absorption with flaxen fiber is ventilative, bacteriostatic deodorizing, antistatic, anti-ultraviolet function, the comfortable soft natural environmental-protective function also with cotton fiber;The invention meets the demand of client, and considerable economic benefit is also brought for enterprise.

Description

Containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton
Technical field
The invention belongs to textile technology field, and in particular to containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton.
Background technology
Hemp is a kind of natural fiber, with good humidity absorption and release, bacteria resistance, the production made of hemp Product ventilation and perspiration function, anti-mould and anti-moth has no stimulation to human body skin, possesses good market prospects.But hemp is in itself There is a situation where that fiber length uniformity is poor, spin Yarn Evenness and filoplume is undesirable, cause existing hemp spinning process bad adaptability, spin The Yarn filoplume gone out is long, and strength is low, and slubbing is more, it is difficult to produce the fiber crops/cotton blending yarn for adapting to high-end customer demand.
The content of the invention
The problem of existing for prior art, it is short, strong it is an object of the invention to design a kind of stable yield of offer, filoplume Power is high, the technical scheme of the technique of the dry uniform fiber crops/cotton blend high-quality yarn that can be adapted to high-end customer demand of bar.
It is described containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton, it is including following dewing, blowing, cotton carding, pre- And, coiled, combing, end simultaneously, rove, spun yarn and winding procedure, it is characterised in that hemp and cotton fiber material are taken, to hemp Fiber is carried out to wet process, then in the public fixed Eight-Diagram of 55/ cotton of ratio hemp 45 arrangement of weighing that gets damp again, 528 are made through cotton cleaning process Grams m lap, then through cotton carding, it is pre- simultaneously, in rolls, combing, end simultaneously, rove, spun yarn, winding procedure produce it is fine containing hemp/cotton The scribbled of dimension, through determining the content of hemp with dyeing-extinction method between 53.5%-50.6%.
It is described containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton, it is characterised in that described hemp For northern river flaxen fiber, described cotton fiber is Xinjiang medium staple cotton, the fineness of cotton fiber material is 4.2, containing it is miscellaneous be 1.60%, short flannel It is 8.07% for 14.2%, regain.
It is described containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton, it is characterised in that described hemp Dewing treatment conditions are:Lubricating oils is by weight 1:10 are watered and are configured to finish, are in hemp weight and finish ratio 20:1, to hemp spraying humidification, 7 centimetres of hemp, one layer of heap finish is humidified once, 1 meter of heap height of embankment, to well wet with thin Film turns over pile 1 time after covering 24 hours, then packing of weighing after 24 hours is stand-by, it is ensured that hemp regain is more than 15%.
It is described containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton, it is characterised in that described cotton cleaning process The middle 002 griping cotton machine hired roughneck blade used is saw blade shape, and blade is concordant with rib, 890 revs/min of hired roughneck's rotating speed, dolly lifting Using VFC, dolly running efficiency more than 90%, cotton-pressing curtain and the brad curtain gauge of mixed cotton slitter are controlled at 30 millimeters, the One 480 revs/min of Beater Speed, the second 780 revs/min of Beater Speed falls miscellaneous 90 ° of dirt rod, opener hired roughneck is beaten using nose-shaped 450 revs/min of hand speed, falls miscellaneous 45 ° of dirt rod, and the leaf blade kirschner beater of lapper three, 920 revs/min of Beater Speed falls miscellaneous dirt 90 ° of rod, 10 revs/min of compacting roller, 4 pure cotton rove interval laps layers of headstock extension, 528 grams of hemp/cotton fiber blend lap/ Rice.
It is described containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton, it is characterised in that described carding step Middle 330 revs/min of breast swift rotating speed, 770 revs/min of licker-in, 12 revs/min of doffer, the cm per minute of removable cover 15, Licker-in divides comb double dust collection knife YESB186 type bottom drains, the concordant 90 degree of gauges 19 English silk of the first mote knife, the second mote knife import in advance The English of gauge 17 silk, cylinder and the English of doffer's gauge 5 silk, cylinder is respectively 11,9,9,9,10 English silk, tin with 5 gauges of removable cover It is 15 English silk that woods is suitable for reading with rear cowl, and suitable for reading with front knife plate is 28 English silk, and doffer is 12 English silk, weight with transfer roller gauge The tooth of gear 15, pushes the tooth of roller gear 19,104.1 times of drafting multiple, 25.3 ± 0.4 grams/5 meters of carded sliver weight.
It is described containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton, it is characterised in that described pre- and process Middle to use 5 and close, 8.79 times of total draft multiple, roller gauge 5 × 15,300 revs/min of front roller rotating speed, shaping is quantitative 14.5 grams/5 meters.
It is described containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton, it is characterised in that described combing process Middle 100 beats/min of combing pincers time, JX-4C-201 type saw whole cylinders, JF201-00D type integrated top combs, 10 lis of detaching distance Rice, nipper and the English of cylinder gauge 15 silk, shaping are quantitative 20.5 grams/5 meters.
It is described containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton, it is characterised in that described Roving Frames It is quantitative 4.5 grams/10 meters using 128 twist factors.
It is described containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton, it is characterised in that described spinning process Using match network negative pressure collecting spinning process, 65 ° of rollers 1 of polyurethane:18 porous coatings, gather the handkerchief of negative-pressure air-suction 3200.
It is described containing 52 hemps/48 natural fiber mixed yarn spinning process of cotton, it is characterised in that described winding procedure Using SAVIO-XCL type bobbin-winding machines, network phenanthrene ZENIT photoelectric-type electronic yarn clearers, Mei Si wears 690 air splicers, winding speed 900 revs/min.
By using above-mentioned technology, compared with prior art, the method have the advantages that:
1)In dewing process by increasing the regain of hemp to wet process to hemp, strengthen the strength of hemp, improve hemp Spinnability.
2)Blowing row bag is made mixing more uniform, proportioning is correct, reduced not in the public fixed ratio Eight-Diagram arrangement of weighing that gets damp again Necessary loss.
3)Carding step leads cotton device from web boundling, improves the yield of carding machine, prevents web phenomenon, improves Row yielding.
4)JX-4C-201 type saw whole cylinders, JF201-00D type integrated top combs, detaching distance are used in combing process 10 centimetres, nipper and cylinder gauge 15 English silk technique remove cotton knot, short flannel, impurity and the waste of flax in the carded sliver, made spun mixed The lines that spin are dry uniform, and filoplume is short, and strength is high, submissive using the thread fabric feeling of the mixed yarn, and moisture absorption is breathed freely, antibacterial anti- It is smelly.
Instant invention overcomes the spinning process that hemp is not suitable with cotton spinning process, hemp is substantially increased in blending Content ratio in yarn, make the fabric of hemp/cotton blended yarn not only the moisture absorption with flaxen fiber be ventilative, bacteriostatic deodorizing, it is antistatic, Anti-ultraviolet function, the comfortable soft natural environmental-protective function also with cotton fiber;The invention meets the demand of client, is also enterprise Industry brings considerable economic benefit.
Embodiment
The invention will be further described with reference to embodiments:
Embodiment 1:Produce the 18.20tex aggregation match network scribbleds of 52/ cotton of hemp 48
Cotton fiber uses Xinjiang medium staple cotton, 27.5 millimeters of average length, fineness 4.2, containing miscellaneous 1.60%, short flannel 14.2%, regain 8.07%, hemp is using northern river flaxen fiber, 29.9 millimeters of average length.
Operating process:
Dewing process:Lubricating oils presses 1:10 are watered, and hemp weight and finish ratio are 20:1, use compressed air aerosolizer Uniform to give hemp humidification, 7 centimetres of hemp, one layer of heap finish is humidified once, and stacking is about high 1 meter, to well wet with thin Film covering health turns over pile 1 time after 24 hours, then packing of weighing after health in 24 hours is stand-by.
Cotton cleaning process:By bag-packaged hemp and cotton fiber in public fixed Eight Diagrams of 55/ cotton of ratio hemp 45 of weighing that get damp again Figure arrangement, because waste of flax is more in hemp, therefore throws 3%, heap bag is accomplished to cut high joint filling more hemp in charge ratio, use A002 type disc bale pluckers, griping cotton machine hired roughneck blade is saw blade shape, and blade is concordant with rib, 890 revs/min of hired roughneck's rotating speed.It is small Car lifting uses VFC, dolly running efficiency more than 90%.1.8 ms/min of the cotton transport curtain speed of SFA035C mixed cotton slitters, Cotton-pressing curtain and brad curtain gauge are controlled at 30 millimeters, the first 480 revs/min of Beater Speed, the second 780 revs/min of Beater Speed, Fall miscellaneous 90 ° of dirt rod, 800 revs/min of porcupine cutter speed.FA106 openers hired roughneck use nose-shaped hired roughneck, 450 revs/min of speed, Fall 8 millimeters of miscellaneous 45 ° of dirt rod, hired roughneck and feed roll motor gauge.54 ms/min of SF161 vibration cotton feeder brad curtains speed, feeds cotton sieve 5.81 revs/min of drawing, evener roller and oblique 25 millimeters of curtain gauge, the leaf blade kirschner beater of A076E lappers three, Beater Speed 920 revs/min, 8 millimeters of hired roughneck and pedal roller gauge fall miscellaneous 90 ° of dirt rod, 10 revs/min of compacting roller, headstock hang 4 it is pure Cotton rove interval lap layer, prevents cotton carding from producing viscous volume, 28.2 meters of lap computational length, every meter of 530 grams of weight during debatching.
Carding step:330 revs/min of A186H breast swifts rotating speed, Bearded-needle knitted cloth selects AC2030S × 1740D, thorn 770 revs/min of roller, taker-in clothing selects AT5010 × 05032VP, feed plate and licker-in gauge 18 English silk, the tooth of weight gear 15, 12 revs/min of doffer speed, doffer's pin cloth selects AD4030 × 01890P, cylinder and the English of doffer's gauge 5 silk, 15 lis of removable cover M/min, revolving tops select MCH42D types, and cylinder and 5 gauges of removable cover are respectively 11,9,9,9,10 English Silk..Licker-in precarding board double dust collection knife YESB186 type bottom drains, the concordant 90 degree of gauges 19 English silk of the first mote knife, the second dedusting The English of knife import gauge 17 silk.Securing cover plate selects GFB300C band crosrol web cleaners, cylinder and the English of back fixed flat setting 12 silk, Cylinder and rear cowl suitable for reading are 15 English silk, and suitable for reading with front knife plate is 28 English silk, cylinder and preceding 3 gauges of securing cover plate are 9,8, 9 English silk.Doffer is 12 English silk with transfer roller gauge;Shaping pushes the tooth of roller gear 19.104.1 times of drafting multiple.Carded sliver weight 25.3 ± 0.4 grams/5 meters.Because the more cohesive force of hemp proportioning is poor, cotton device is led from web boundling.
Pre- and process:FA306 drawing frames are using 5 and close, 8.79 times of total draft multiple, roller gauge 5 × 15, front roller 300 revs/min of rotating speed, drafting rubber roller selects WAC-GB78, the double group osmosis types 1 of RC-AB types:8 coating.Quantitatively 14.5 grams of shaping/ 5 meters.Along Draft Configuration, using 3 play pressure bar preliminary draft techniques on 4, increase Fiber Straightness, is that combing process is ready work Make
Coiled process:SFA332 lappers are using 20 and close, 1.305 times of total draft multiple, are conducive to road after improving to comb effect Really, the tooth of fixed length gear 30,113 meters of examination paper length, the grams m of examination paper weight 42.
Combing process:SFA252A combing machines use JX-4C-201 type saw whole cylinders, cylinder and the English of nipper gauge 15 Silk, JF201-00D type integrated top combs, top comb separates 0.75 millimeter of roller gauge with after, and top comb passes in and out gauge 1 with rear detaching roller Millimeter, -2.5 millimeters of height gauge, 10 centimetres of detaching distance removes cotton knot, short flannel, impurity and the waste of flax in the carded sliver, feeds cotton Several 4 teeth of tooth are supportted, the tooth of cotton sheet powershift gear 48, the tooth of feed roll motor ratchet 12, the tooth of web tension force gear 81, table top bar tension force gear 41 is fed Tooth, cambered plate positioning 2 is indexed, and nipper front position positioning 19 is indexed, and the clockwise timing 9 of detaching roller is indexed, clamp plate closure timing 28.5 indexing, noil disk 14 is indexed, the pincers beat/min of cylinder speed 110.20.1 grams/5 meters of shaping weight.
End and process:FA306 end and process in two roads and close 8.1 times, 8 of drawing frame total draft multiple and close, roller Gauge 3 × 12,200 revs/min of front roller rotating speed, drafting rubber roller selects WAC-GB78, the double group osmosis types 1 of RC-AB types:10 apply Material.Shaping is quantitative 20 grams/5 meters.
Slubbing process:FA458A fly frames use the roller draft structure of double-short leather-ring Spring cradle four, above and below WRA-S-5 glue Circle, WRC-975 rubber rolls, the roller gauge of drawing-off four is 9 × 22 × 26,800 revs/min of flier rotating speed, back zone drafting multiple 1.19 Times, 1.048 times of bar tension draft multiple is fed, roving twist factor 128,4.5 grams/10 meters of regular roving feeding increases the cohesive force of rove, Reduce misdraft.
Spinning process:FA506 spinning frames, which are used, matches network negative pressure collecting spinning process, TK142 Spring cradles, length apron, Xiao on the type list pressure bars of 6833B VI, drafting roller gage 17.8 × 28,1.254 times of back zone drafting multiple, upper glue roller guide, it is preceding, In, rear fourth gear pressure be respectively 90,175,115,130 newton, brilliant coloured silk 65 ° of rollers 1 of polyurethane:18 porous coatings, gather negative The handkerchief of air draught 3200 is pressed, from 120 × 131 × 23.5 grid rings, PG1-4254 alloy steel collars, the UL udr 3/0 of cloth rake C 1 Wire loop, reduces the growth of filoplume, improves spinning yarn quality.
Winding procedure:SAVIO-XCL type bobbin-winding machines, network phenanthrene ZENIT photoelectric-type electronic yarn clearers, Mei Si wears 690 air Splicer, 900 revs/min of winding speed controls the increase of filoplume.
Spinning yarn quality such as following table:(The 18.20tex of 52/ cotton of hemp 48)
Bar is done(CVm) - 50% details + 50% slubbing + 200% cotton is saved 4 millimeters of filoplumes 5 millimeters of filoplumes Strongly
RING SPINNING technique 21.53 157 1305 1409 4.53 2.5 204.1
Present invention process 20.74 122 1184 1376 3.03 1.4 223.2
Above-described embodiment is only one of presently preferred embodiments of the present invention, and the practical range of the present invention is not limited with this, so this The protection domain of invention is simultaneously not only limited with this.

Claims (10)

1. containing the natural fiber mixed yarn spinning process of cotton of 52 hemps/48, including following dewing, blowing, cotton carding, it is pre- simultaneously, in rolls, Combing, end simultaneously, rove, spun yarn and winding procedure, it is characterised in that take hemp and cotton fiber material, hemp carried out To wet process, then in the public fixed Eight-Diagram of 55/ cotton of ratio hemp 45 arrangement of weighing that gets damp again, 528 grams m cottons are made through cotton cleaning process Volume, then through cotton carding, it is pre- simultaneously, in rolls, combing, end simultaneously, rove, spun yarn, winding procedure produce the blending of the fiber containing hemp/cotton Yarn, through determining the content of hemp with dyeing-extinction method between 53.5%-50.6%.
2. as claimed in claim 1 containing the natural fiber mixed yarn spinning process of cotton of 52 hemps/48, it is characterised in that described Hemp is northern river flaxen fiber, and described cotton fiber is Xinjiang medium staple cotton, and the fineness of cotton fiber material is 4.2, is containing miscellaneous 1.60%th, short flannel is that 14.2%, regain is 8.07%.
3. as claimed in claim 1 containing the natural fiber mixed yarn spinning process of cotton of 52 hemps/48, it is characterised in that described Hemp dewing treatment conditions are:Lubricating oils is by weight 1:10 are watered and are configured to finish, by hemp weight and oil Agent ratio is 20:1, to hemp spraying humidification, 7 centimetres of hemp, one layer of heap finish is humidified once, and 1 meter of heap height of embankment is given It is good it is wet covered 24 hours with film after turn over pile 1 time, then packing of weighing after 24 hours is stand-by, it is ensured that hemp regain exists More than 15%.
4. as claimed in claim 1 containing the natural fiber mixed yarn spinning process of cotton of 52 hemps/48, it is characterised in that described The 002 griping cotton machine hired roughneck blade used in cotton cleaning process is saw blade shape, and blade is concordant with rib, 890 revs/min of hired roughneck's rotating speed, Dolly lifting uses VFC, and dolly running efficiency more than 90%, cotton-pressing curtain and the brad curtain gauge of mixed cotton slitter are controlled 30 Millimeter, the first 480 revs/min of Beater Speed, the second 780 revs/min of Beater Speed falls miscellaneous 90 ° of dirt rod, and opener hired roughneck uses 450 revs/min of nose-shaped Beater Speed, falls miscellaneous 45 ° of dirt rod, the leaf blade kirschner beater of lapper three, 920 revs/min of Beater Speed, Fall miscellaneous 90 ° of dirt rod, 10 revs/min of compacting roller, headstock hangs 4 pure cotton rove interval lap layers, hemp/cotton fiber blend lap 528 grams ms.
5. as claimed in claim 1 containing the natural fiber mixed yarn spinning process of cotton of 52 hemps/48, it is characterised in that described 330 revs/min of breast swift rotating speed in carding step, 770 revs/min of licker-in, 12 revs/min of doffer, 15 lis of removable cover M/min, licker-in divides comb double dust collection knife YESB186 type bottom drains in advance, the concordant 90 degree of gauges 19 English silk of the first mote knife, and second removes The English of dirt knife import gauge 17 silk, cylinder and the English of doffer's gauge 5 silk, cylinder and 5 gauges of removable cover are respectively 11,9,9,9,10 English silk, it is 15 English silk that cylinder is suitable for reading with rear cowl, and suitable for reading with front knife plate is 28 English silk, and doffer is 12 English with transfer roller gauge Silk, the tooth of weight gear 15 pushes the tooth of roller gear 19,104.1 times of drafting multiple, 25.3 ± 0.4 grams/5 meters of carded sliver weight.
6. as claimed in claim 1 containing the natural fiber mixed yarn spinning process of cotton of 52 hemps/48, it is characterised in that described 5 are used in pre- and process and is closed, 8.79 times of total draft multiple, roller gauge 5 × 15,300 revs/min of front roller rotating speed goes out Bar is quantitative 14.5 grams/5 meters.
7. as claimed in claim 1 containing the natural fiber mixed yarn spinning process of cotton of 52 hemps/48, it is characterised in that described 100 beats/min of combing pincers time, JX-4C-201 type saw whole cylinders, JF201-00D type integrated top combs, noil in combing process 10 centimetres of gauge, nipper and the English of cylinder gauge 15 silk, shaping are quantitative 20.5 grams/5 meters.
8. as claimed in claim 1 containing the natural fiber mixed yarn spinning process of cotton of 52 hemps/48, it is characterised in that described Roving Frames use 128 twist factors, quantitative 4.5 grams/10 meters.
9. as claimed in claim 1 containing the natural fiber mixed yarn spinning process of cotton of 52 hemps/48, it is characterised in that described Spinning process is using match network negative pressure collecting spinning process, 65 ° of rollers 1 of polyurethane:18 porous coatings, gather negative-pressure air-suction 3200 Handkerchief.
10. as claimed in claim 1 containing the natural fiber mixed yarn spinning process of cotton of 52 hemps/48, it is characterised in that described Winding procedure use SAVIO-XCL type bobbin-winding machines, network phenanthrene ZENIT photoelectric-type electronic yarn clearers, Mei Si wear 690 air twist with the fingers tie Device, 900 revs/min of winding speed.
CN201710431894.3A 2017-06-09 2017-06-09 Spinning process of blended yarn containing 52 hemp/48 cotton natural fibers Active CN107190380B (en)