CN107081827A - A kind of the preservation of timber against decay processing method - Google Patents

A kind of the preservation of timber against decay processing method Download PDF

Info

Publication number
CN107081827A
CN107081827A CN201710290530.8A CN201710290530A CN107081827A CN 107081827 A CN107081827 A CN 107081827A CN 201710290530 A CN201710290530 A CN 201710290530A CN 107081827 A CN107081827 A CN 107081827A
Authority
CN
China
Prior art keywords
timber
soak
preservative
preservation
processing method
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201710290530.8A
Other languages
Chinese (zh)
Inventor
陈熙悌
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Guangxi Qinzhou Cendant Commerce Co Ltd
Original Assignee
Guangxi Qinzhou Cendant Commerce Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Guangxi Qinzhou Cendant Commerce Co Ltd filed Critical Guangxi Qinzhou Cendant Commerce Co Ltd
Priority to CN201710290530.8A priority Critical patent/CN107081827A/en
Publication of CN107081827A publication Critical patent/CN107081827A/en
Pending legal-status Critical Current

Abstract

The invention discloses a kind of the preservation of timber against decay processing method, after herbal medicine immersion liquid disinfection and deinsectization, timber is handled using using full-cell process;The preservative solute used in processing procedure is ACC or CDDC, and solvent is above-mentioned herbal medicine immersion liquid;Finally wood surface after the drying applies last layer whether-resisting wood oil, that is, completes preservative treatment.Chinese prickly ash, wrinkled giant hyssop and ginkgo leaf are common Chinese medicine, the effect with disinfection and deinsectization;Then preservative treatment is carried out with full-cell process, makes between gap of the preservative full of timber, play antisepsis, finally can completely cut off air to a certain extent in wood surface brush last layer whether-resisting wood oil again, prevent wood surface from aoxidizing.It can farthest delay the corruption speed of timber after handling timber using this method.

Description

A kind of the preservation of timber against decay processing method
Technical field
The present invention relates to building material field, the seemingly processing method of particularly a kind of timber.
Background technology
Timber is the plant for being capable of secondary growth, such as tree and shrubs, the lignified tissue formed, and these plants are first After raw growth terminates, the vascular cambium in rhizome comes into play, and outwards develops bast, inwardly develops timber.Timber is Common building and finishing material, are traditional construction materials, extensive use are obtained in ancient building and modern architecture, in knot On structure, timber is mainly used in framework and roof, such as beam, post, rafter, roof boarding, sets of brackets on top of the columns, and timber is always widely used in building Interior decoration and decoration, it gives the enjoyment of natural beauty, moreover it is possible to the interior space is produced warm and cordial feeling, such as bar timber floor It is indoor using most common wood floor, it is made up of the part such as keel, floor.But influenceed, held by timber self character Easily occurred the change such as discoloration, rotten by the effect of environment (sunlight, oxygen, moisture temperature etc.) and microorganism (fungi), cause wood Material softens, and every intensity step-down easily caves in, so the preservation of timber against decay processing is the key that timber is used as building materials.By anti- The timber of corruption processing possesses corrosion resistant advantage, therefore is particularly suitable for use in various outdoor architectures, and such as gardens wayside pavilion landscape, waterside pavilion are returned Corridor, flower stand fences, wooden footway etc..
The content of the invention
In view of the deficienciess of the prior art, it is an object of the invention to provide a kind of the preservation of timber against decay processing method, effectively Prevent foxiness, the service life of prolonging wood.
In order to achieve the above object, the technical scheme that the present invention is provided is as follows:
A kind of the preservation of timber against decay processing method, comprises the following steps:
1) Chinese prickly ash, wrinkled giant hyssop, ginkgo leaf are put into water by weight 1: 2: 1, after immersion 30-40min, with small fire infusion 5- 8h, obtains deinsectization sterilization soak, soak is poured into fermentation vat, timber is fully immersed in soak, soak is treated When being cooled to room temperature, sodium fluoride and Tea Saponin are added in soak, 15-60h is soaked;
2) by step 1) in soak after timber be placed in that to dry place air-dried;
3) using full-cell process process step 2) in the timber that air-dries;Used in processing procedure and arrive preservative, the anti-corrosion Agent is by step 1) described in soak and ACC or CDDC mixing constitute;
4) by step 3) in treat after timber be put into dryer, dried at a temperature of 90-200 DEG C, until timber contains Water is no more than 8%;Normal temperature is cooled to after drying, one layer of whether-resisting wood oil is uniformly coated with wood surface.
Further, step 3) full-cell process concretely comprise the following steps:Timber is put into after process tank and vacuumized, vacuum It is not less than 80kPa, keeps adding preservative after vacuum 20-60min under vacuum, preservative, which is filled up after process tank, releases true Sky, and start pressurization, holding pressure is 1-1.5MPa, until the anti-corrosion dosage in process tank is no longer reduced.
Further, the preservative is prepared as the soak described in ACC/CDDC and step one by weight 1: 1-1.5.
Further, step 1) in sodium chloride and Tea Saponin addition be 10-50g/L soaks.
Beneficial effects of the present invention:Chinese prickly ash, wrinkled giant hyssop and ginkgo leaf are common Chinese medicine, the effect with sterilization, Sterilized before wood preservation processing, can kill wood internal microorganism that may be present and worm's ovum etc. can accelerate timber Rotten factor;Then preservative treatment is carried out with full-cell process, makes between gap of the preservative full of timber, play anti-corrosion work With finally can completely cutting off air to a certain extent in wood surface brush last layer whether-resisting wood oil again, prevent wood surface oxygen Change.It can farthest delay the corruption speed of timber after handling timber using this method.
Embodiment
The following specific embodiments are described below is described in further detail to the present invention.
Embodiment 1
Thickness is less than 50mm timber, and preservative treatment is carried out using following steps:
1) Chinese prickly ash, wrinkled giant hyssop, ginkgo leaf are put into water by weight 1: 2: 1, after immersion 35min, with small fire infusion 8h, obtained Soak is sterilized to deinsectization, soak is poured into fermentation vat, timber is fully immersed in soak, treats that soak is cooled to During room temperature, sodium fluoride and Tea Saponin are added in soak, the addition of sodium chloride and Tea Saponin is 10g/L, soaks 15h;
2) by step 1) in soak after timber be placed in that to dry place air-dried;
3) timber is put into after process tank and vacuumized, until vacuum reaches 80kPa, kept after vacuum 20min in vacuum Under the conditions of add preservative, preservative fills up and vacuum is released after process tank, and start pressurization, holdings pressure be 1MPa, until locate Anti-corrosion dosage in reason tank is no longer reduced;The preservative solute used in processing procedure be ACC, solvent be step 1) described in leaching Steep liquid;
4) by step 3) in treat after timber be put into dryer, dried at a temperature of 90 DEG C, until timber water content No more than 8%;Normal temperature is cooled to after drying, one layer of whether-resisting wood oil is uniformly coated with wood surface.
Embodiment 2
Thickness carries out preservative treatment in the timber of 50-120mm scopes using following steps:
1) Chinese prickly ash, wrinkled giant hyssop, ginkgo leaf are put into water by weight 1: 2: 1, after immersion 35min, with small fire infusion 8h, obtained Soak is sterilized to deinsectization, soak is poured into fermentation vat, timber is fully immersed in soak, treats that soak is cooled to During room temperature, sodium fluoride and Tea Saponin are added in soak, the addition of sodium chloride and Tea Saponin is 20g/L, soaks 30h;
2) by step 1) in soak after timber be placed in that to dry place air-dried;
3) timber is put into after process tank and vacuumized, until vacuum reaches 80kPa, kept after vacuum 25min in vacuum Under the conditions of add preservative, preservative fills up and vacuum is released after process tank, and start pressurization, holdings pressure be 1MPa, until locate Anti-corrosion dosage in reason tank is no longer reduced;The preservative solute used in processing procedure be ACC, solvent be step 1) described in leaching Steep liquid;
4) by step 3) in treat after timber be put into dryer, dried at a temperature of 95 DEG C, until timber water content No more than 8%;Normal temperature is cooled to after drying, one layer of whether-resisting wood oil is uniformly coated with wood surface.
Embodiment 3
Thickness is more than 120mm timber, and preservative treatment is carried out using following steps:
1) Chinese prickly ash, wrinkled giant hyssop, ginkgo leaf are put into water by weight 1: 2: 1, after immersion 40min, with small fire infusion 8h, obtained Soak is sterilized to deinsectization, soak is poured into fermentation vat, timber is fully immersed in soak, treats that soak is cooled to During room temperature, sodium fluoride and Tea Saponin are added in soak, the addition of sodium chloride and Tea Saponin is 50g/L, soaks 50h;
2) by step 1) in soak after timber be placed in that to dry place air-dried;
3) timber is put into after process tank and vacuumized, until vacuum reaches 80kPa, kept after vacuum 35min in vacuum Under the conditions of add preservative, preservative fills up and vacuum is released after process tank, and start pressurization, holdings pressure be 1.2MPa, up to Anti-corrosion dosage in process tank is no longer reduced;The preservative solute used in processing procedure is ACC, and solvent is step 1) described in Soak;
4) by step 3) in treat after timber be put into dryer, dried at a temperature of 100 DEG C, until timber water content No more than 8%;Normal temperature is cooled to after drying, one layer of whether-resisting wood oil is uniformly coated with wood surface.
Described above is only the preferred embodiment of the present invention, is not the limitation to the scope of the claims of the present invention, all to belong to Technical scheme under thinking of the present invention belongs to protection scope of the present invention.It should be pointed out that for the ordinary skill people of this area For member, some improvements and modifications without departing from the inventive concept of the premise, these improvements and modifications also should be regarded as this hair Bright protection domain.

Claims (4)

1. a kind of the preservation of timber against decay processing method, it is characterised in that comprise the following steps:
1) Chinese prickly ash, wrinkled giant hyssop, ginkgo leaf are put into water by weight 1: 2: 1, after immersion 30-40min, with small fire infusion 5-8h, Deinsectization sterilization soak is obtained, soak is poured into fermentation vat, timber is fully immersed in soak, treats that soak is cooled down During to room temperature, sodium fluoride and Tea Saponin are added in soak, 15-60h is soaked;
2) by step 1) in soak after timber be placed in that to dry place air-dried;
3) using full-cell process process step 2) in the timber that air-dries;In processing procedure use arrive preservative, the preservative by Step 1) described in soak and ACC or CDDC mixing composition;
4) by step 3) in treat after timber be put into dryer, dried at a temperature of 90-200 DEG C, until timber water content No more than 8%;Normal temperature is cooled to after drying, one layer of whether-resisting wood oil is uniformly coated with wood surface.
2. a kind of the preservation of timber against decay processing method according to claim 1, it is characterised in that step 3) full-cell process Concretely comprise the following steps:Timber is put into after process tank and vacuumized, vacuum is not less than 80kPa, is kept after vacuum 20-60min true Preservative is added under empty condition, preservative fills up and vacuum is released after process tank, and starts pressurization, holding pressure is 1-1.5MPa, Until the anti-corrosion dosage in process tank is no longer reduced.
3. a kind of the preservation of timber against decay processing method according to claim 1, it is characterised in that the preservative is by ACC/ CDDC and the soak described in step one are prepared by weight 1: 1-1.5.
4. a kind of the preservation of timber against decay processing method according to claim 1, it is characterised in that step 1) in sodium chloride and tea The addition of saponin is 10-50g/L soaks.
CN201710290530.8A 2017-04-27 2017-04-27 A kind of the preservation of timber against decay processing method Pending CN107081827A (en)