CN106290147B - Rubber pad rubber adhesive strength test method - Google Patents

Rubber pad rubber adhesive strength test method Download PDF

Info

Publication number
CN106290147B
CN106290147B CN201610581146.9A CN201610581146A CN106290147B CN 106290147 B CN106290147 B CN 106290147B CN 201610581146 A CN201610581146 A CN 201610581146A CN 106290147 B CN106290147 B CN 106290147B
Authority
CN
China
Prior art keywords
rubber
metallic plate
hole
rubber pad
layer
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201610581146.9A
Other languages
Chinese (zh)
Other versions
CN106290147A (en
Inventor
刘鹏
易伟球
王林
谢彦飞
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Zhuzhou Times New Material Technology Co Ltd
Original Assignee
Zhuzhou Times New Material Technology Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Zhuzhou Times New Material Technology Co Ltd filed Critical Zhuzhou Times New Material Technology Co Ltd
Priority to CN201610581146.9A priority Critical patent/CN106290147B/en
Publication of CN106290147A publication Critical patent/CN106290147A/en
Application granted granted Critical
Publication of CN106290147B publication Critical patent/CN106290147B/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

Rubber pad rubber adhesive strength test method, with the rubber layer between vertical force-extension adjacent two layers metallic plate, until rubber layer is detached from metallic plate, vertical external force F when metallic plate and rubber layer are detached from and when testing metallic plate and rubber layer bond area S, the ratio for calculating F and S is worth to the adhesive strength P of rubber layer and metallic plate, adjacent two layers metallic plate is upper layer metallic plate and lower metal plate, the upper pressure hole being vertically staggered is opened up on rubber pad and pushes hole, upper pressure hole and pushing Kong Zhongjun are inserted into round steel, move downward the round steel in upper pressure hole under the action of vertical external force, upper layer metallic plate and lower metal plate distance increase, stretch the rubber layer between upper layer metallic plate and lower metal plate, until upper layer metallic plate and/or lower metal plate and rubber layer with detach.The present invention tests the adhesive strength of metallic plate in rubber pad and rubber layer according to the design feature of rubber pad, and test philosophy is simple, and test operation is simple, and testing reliability is high.

Description

Rubber pad rubber adhesive strength test method
Technical field
The present invention relates to a kind of rubber pad rubber adhesive strength test methods, are used for test tracks traffic vibration insulating system Rubber damping pad in rubber and metallic plate adhesive strength.
Background technology
Rubber product is more and more widely used in fields such as locomotive, automobile, oil exploitations, and rubber has certain tension It stretches, the performance of wear-resisting and tear-resistant intensity, and also wants that good elasticity can be kept for a long time under cryogenic, with high-speed rail The fast development of road traffic is continuously increased the demand of rubber, meanwhile, it is also increasingly harsher to the performance requirement of rubber, Especially to the adhesive property of metal-rubber product, more stringent requirements are proposed.Metal and rubber in the vibration insulating system of rail traffic Vulcanize the rubber pad formed, use is quite extensive.The vibration damping that the adhesive strength of metal and rubber directly influences rubber pad is reliable Property and service life.
National standard GB/T15254-2014,《Vulcanized rubber and 180 ° of disbonded tests of metal adhesive》Metal and vulcanized rubber are shelled Measurement Method from intensity is provided, will be vertically arranged by vulcanized rubber and sample made of metal adhesive, in sample Open end is parallelly gradually removed along the length direction for being glued material with stable speed, and the power of application is by rubber by viscous material The released part of material, and it is parallel to metallic plate, can bear on sample unit width is strong for 180 ° of strippings by equal peeling force Degree.Peel strength, that is, rubber in above-mentioned national standard adhesive strength Nian Jie with metal sheet plane.In this way, by metallic plate with Rubber is removed, it is necessary to fixture be respectively set in the end that metallic plate and rubber do not bond together, pulled and pressed from both sides by external force Tool keeps metallic plate peeling-off with rubber.And the rubber pad used in rail traffic vibration insulating system, generally metal and rubber sulphur Chemical conversion is whole, metal with do not have the end that can be clamped by fixture in rubber, method specified in GB/T1524-2014 is simultaneously Be not suitable for carrying out disbonded test to above-mentioned rubber pad.
It is entitled application No. is 201310087901.4《Lamp bracket rubber adhesive strength testing machine structure》Invention it is special Profit discloses a kind of lamp bracket rubber adhesive strength testing machine structure, and lamp bracket is component to be tested, by upper plate, lower plate It is bonded and forms with rubber bodies, the rubber bodies in component to be tested are stretched with upper member and lower member, make rubber bodies and metallic plate point From wherein upper member is fixedly connected with upper plate in component to be tested, and lower member is fixedly connected with the lower plate in component to be tested, is led to It crosses test equipment and pulls upper member and lower member movement, upper plate and lower plate movement is driven to stretch rubber bodies.Above-mentioned patent is also fortune With the design feature of lamp bracket, upper member is made to be connect with upper plate, lower member is connect with lower plate, and rubber bodies are stretched to reach Purpose.And its structure of the rubber pad used in traffic track and lamp bracket and differ, it cannot be with upper member and lower member shape At being fixedly connected, the technical solution in foregoing invention patent applies in rubber pad, upper member and lower member and rubber can not be made Metallic plate in rubber cushion is affixed, and the purpose for testing out rubber adhesive strength is difficult to reality.
About the test method of rubber adhesive strength all it is in the prior art as a result, the design feature according to sample to be tested Come what is tested, but there is no the test methods or test equipment that are directed to rubber gasket structure, and the present invention is i.e. according to rubber pad Design feature provides a kind of rubber pad rubber adhesive strength test method.
Invention content
The present invention provides a kind of rubber pad rubber adhesive strength test method according to the design feature of rubber pad, hands over track The adhesive strength of metallic plate and rubber layer is tested in rubber pad in logical vibrational system, and test philosophy is simple, test operation Simply, testing reliability is high.
The technical solution adopted by the present invention is in order to achieve the above objectives:Rubber pad rubber adhesive strength test method, selection Round rubber pad or polygon rubber pad are tested, and each layer metallic plate and the bond area of rubber layer are equal in rubber pad, Rubber pad is horizontally disposed with, with the rubber layer between vertical force-extension adjacent two layers metallic plate, until rubber layer and metallic plate Be detached from, vertical external force F when metallic plate and rubber layer are detached from and when test metallic plate and rubber layer bond area S, count The ratio for calculating F and S is worth to the adhesive strength P of rubber layer and metallic plate, it is characterised in that the adjacent two layers metallic plate difference For upper layer metallic plate and lower metal plate, opened up on the rubber pad be vertically staggered and upper pressure hole that diameter is equal and under Hole is pressed, the upper pressure hole is opened up across upper layer metallic plate from the top surface of rubber pad to the top surface of lower metal plate, under described Pressure hole is opened up from the bottom surface of rubber pad across lower metal plate to the bottom surface of upper layer metallic plate, and upper pressure hole and pushing Kong Zhongjun are inserted into Round steel moves downward the round steel in upper pressure hole under the action of vertical external force, and upper layer metallic plate and lower metal plate distance increase Greatly, the rubber layer between upper layer metallic plate and lower metal plate is stretched, until upper layer metallic plate and/or lower metal plate and rubber Layer with detach.
Preferably, the sum of the hole area in upper pressure hole and the sum of the hole area for pushing hole are not less than metallic plate and rubber layer The 1/15 of bond area.
Preferably, the upper pressure hole is equal with the quantity in hole is pushed, and upper pressure hole and pushing hole are uniform on the same circumference Isolation is distributed, and between two adjacent upper pressure holes one pushing hole of distribution.
Preferably, it the upper pressure hole and pushes the area of circumference where pore size distribution to account for metallic plate bonding with rubber layer The 1/3 ~ 1/2 of area.
Preferably, a diameter of 16 ~ 24mm in upper pressure hole, quantity are 4 ~ 8.
Preferably, the length of the round steel is 3 ~ 4 times of rubber mat thickness, between one end of round steel and upper pressure hole or pushing hole Gap coordinates.
Preferably, the round steel being placed in pressure hole connects to form entirety by steel seat, is placed in the circle pushed in hole Steel connects to form entirety also by steel seat, and the steel seat is horizontally disposed parallel with rubber pad, and the steel seat is fixed on round steel The other end, vertical force act on make on steel seat press hole in round steel move downward.
Preferably, the vertical force acted on steel seat is provided by pressure testing machine, the rubber pad is set to pressure On testing machine, the steel seat of the round steel end in upper pressure hole is contacted with the pressure head of pressure testing machine, pushes the round steel end in hole Steel seat is contacted with the chassis of pressure testing machine, and Opening pressure testing machine, pressure head moves downward, and pressure, which acts on steel seat, makes pressure Round steel in hole moves downward, and upper layer metallic plate and lower metal plate distance increase, when upper layer metallic plate and lower metal plate with When rubber layer is with being detached from, the load reading of pressure testing machine is vertical external force F when metallic plate is detached from rubber layer.
Preferably, " the bond area S of metallic plate and rubber layer when test " refers to that upper layer metallic plate is bonding with rubber layer Area subtracts the sum of the hole area in upper pressure hole and pushing hole in rubber pad.
Preferably, when pressure testing machine is opened, the speed control that pressure head moves downward is in 10 ~ 20mm/min.
The present invention opens up the upper pressure hole being vertically staggered on rubber pad and pushes hole according to the design feature of rubber pad, Upper pressure hole is opened up from the top surface of rubber pad across upper layer metallic plate to the top surface of lower metal plate, pushes bottom surface of the hole from rubber pad It opens up across lower metal plate to the bottom surface of upper layer metallic plate, and is applied to upper layer metallic plate and lower metal plate by round steel and hung down Xiang Li makes upper layer metallic plate and lower metal plate pull open, until being detached from rubber layer, tests the metallic plate and rubber layer obtained Adhesive strength error is small, and accuracy rate is high.The present invention carries out trepanning processing to tested rubber pad, and external force is made to may be made directly to gold Belong on plate, test philosophy is simple, and test operating procedure is simple, and testing reliability is high.
Description of the drawings
Fig. 1 is rubber pad, round steel, steel seat and pressure in the rubber pad rubber adhesive strength test method of specific implementation mode The assembly structure figure of testing machine.
Fig. 2 is the distribution map on the upper pressure hole that rubber pad opens up and pushing mono- circumference of Kong Yuan.
Specific implementation mode
It 1 to Fig. 2 elaborates below in conjunction with the accompanying drawings to the embodiment of the present invention.
Rubber pad rubber adhesive strength test method selects round rubber pad or polygon rubber pad to be tested, rubber Each layer metallic plate and the bond area of rubber layer are equal in pad, and rubber pad is horizontally disposed with, with vertical force-extension adjacent two Rubber layer between layer metallic plate, until rubber layer is detached from metallic plate, it is vertical outer when metallic plate is detached from rubber layer Power F and when test metallic plate and rubber layer bond area S, calculating the ratio of F and S, to be worth to rubber layer bonding with metallic plate Intensity P, it is characterised in that the adjacent two layers metallic plate is respectively upper layer metallic plate 100 and lower metal plate 101, described Rubber pad on open up and be vertically staggered and upper pressure hole 1 that diameter is equal and push hole 2, the upper pressure hole 1 is from rubber pad Top surface is opened up across upper layer metallic plate 100 to the top surface of lower metal plate 101, and the pushing hole 2 is opened from the bottom surface of rubber pad If across lower metal plate 101 to the bottom surface of upper layer metallic plate 100, it is inserted into round steel 3 in upper pressure hole 1 and pushing hole 2, vertical Make that the round steel 3 in hole 1 is pressed to move downward under the action of external force, upper layer metallic plate 100 and lower metal plate 101 apart from increase, The rubber layer 102 between upper layer metallic plate 100 and lower metal plate 101 is stretched, until upper layer metallic plate 100 and/or lower layer's gold Belong to plate 101 and rubber layer 102 and detaches.
Above-described rubber pad rubber adhesive strength test method, according to the design feature of rubber pad, on rubber pad Open up the upper pressure hole 1 that is vertically staggered and push hole 2, upper pressure hole 1 from the top surface of rubber pad open up across upper layer metallic plate 100 to The top surface of lower metal plate 101 pushes hole 2 and is opened up from the bottom surface of rubber pad across lower metal plate 101 to upper layer metallic plate 100 Bottom surface, and vertical force is applied to upper layer metallic plate 100 and lower metal plate 101 by round steel 3, makes 100 He of upper layer metallic plate Lower metal plate 101 pulls open, until being detached from rubber layer 102.It should be noted that different with 2 quantity of hole is pushed in upper pressure hole 1 When, upper layer metallic plate 100 and lower metal 101 may be caused not to be detached from rubber layer 102 simultaneously, when upper layer metallic plate 100 with One of them is detached from lower metallic plate 101 with rubber layer 102, just records vertical external force F when metallic plate is detached from rubber layer, you can Calculate the adhesive strength of the metallic plate and rubber layer that are detached from rubber layer.
By multiple repetition test, the sum of the hole area in upper pressure hole 1 and the sum of the hole area for pushing hole 2 are not less than metal The 1/15 of plate and the bond area of rubber layer, it is ensured that metallic plate under the promotion of round steel, can be effectively detached from rubber layer, and circle Steel 3 moves downward that stroke is moderate, avoids the damage of round steel 3 in test process.
Wherein, the upper pressure hole 1 is equal with the quantity in hole 2 is pushed, and upper pressure hole 1 and pushing hole 2 are equal on the same circumference Even isolation is distributed, and between two adjacent upper pressure holes 1 one pushing hole 2 of distribution, as can be seen from Figure 2 upper pressure hole 1 and pushing The quantity in hole 2 is four, and is evenly distributed on same circumference, ensure upper layer metallic plate 100 and lower metal plate 101 by Power is uniform, and upper pressure hole 1 is equal with 2 quantity of hole is pushed, and upper layer metallic plate 100 and lower metal plate 101 can be made same with rubber layer 102 When be detached from.
Wherein, it is bonding with rubber layer to account for metallic plate for the area of the circumference in the upper pressure hole 1 and pushing hole 2 distribution place The 1/3 ~ 1/2 of area, as shown in Figure 2, the area of inner ring A are the area of the circumference where upper pressure hole 1 and the distribution of pushing hole 2, The area of outer ring B is the bond area of metallic plate and rubber layer, i.e. the area of inner ring A accounts for the 1/3 ~ 1/2 of the area of outer ring B, is protected Demonstrate,prove metallic plate plane uniform force Nian Jie with rubber layer, metallic plate is essentially whole face disengaging, raising survey with rubber layer when disengaging The operability of method for testing.
Specifically, a diameter of 16 ~ 24mm in upper pressure hole 1, quantity are 4 ~ 8, upper layer metallic plate 100 and lower metal plate 101 have enough forced areas, and metallic plate is made to be detached from rubber layer, and upper pressure hole 1 and the size sum number for pushing hole 2 Metallic plate and the bond area of rubber layer are too small when amount will not cause to test, to ensure the adhesive strength tested out in error model In enclosing.
In actual test, the length of round steel 3 is too short, can lead to press the round steel 3 in hole and push the round steel in hole 2 3, which collide with each other, causes to damage, long, can improve space requirement when difficulty of test and test, therefore the length of the round steel 3 It is 3 ~ 4 times of rubber mat thickness, can effectively avoid round steel 3 in test process and more collsion damages, one end of round steel 3 and upper pressure occurs Hole 1 pushes 2 clearance fit of hole, facilitates the placement of round steel 3.
Wherein, the round steel 3 being placed in pressure hole 1 is connected by steel seat 4 forms entirety, is placed in and pushes in hole 2 Round steel 3 is connected also by steel seat 4 forms entirety, and the steel seat 4 is horizontally disposed parallel with rubber pad, and the steel seat 4 is fixed In the other end of round steel 3, vertical force, which acts on, makes that the round steel 3 in hole 1 is pressed to move downward on steel seat 4, and steel seat 4 is by 3 side of round steel Even whole, vertical force acts on steel seat 4, makes to press the stress synchronous with the round steel 3 pushed in hole 2 of hole 1, is further ensured that metal The uniform force of plate.
As shown in Figure 1, providing the vertical force acted on steel seat 4, rubber pad setting by pressure testing machine 200 In on pressure testing machine 200, the steel seat 4 of 3 end of round steel in upper pressure hole 1 is contacted with the pressure head of pressure testing machine, is pushed in hole 2 The steel seat 4 of 3 end of round steel contacted with the chassis of pressure testing machine, Opening pressure testing machine, pressure head moves downward, pressure effect Move downward the round steel 3 in upper pressure hole 1 on steel seat 4, upper layer metallic plate 100 and lower metal plate 101 are apart from increase, when upper When layer metallic plate 100 and lower metal plate 101 and rubber layer 102 are with being detached from, the load reading of pressure testing machine be metallic plate with Vertical external force F when rubber layer is detached from.When pressure testing machine is opened, the speed control that pressure head moves downward is in 10 ~ 20mm/ Min, when tester being facilitated accurately to read upper layer metallic plate 100 and lower metal plate 101 with rubber layer 102 and disengaging, pressure The load of testing machine is read.
With above-described rubber pad rubber adhesive strength test method, the rubber adhesive strength of rubber pad is surveyed Examination the specific steps are:
(One)Upper pressure hole 1 is opened up on rubber pad to be measured and pushes hole 2, and the quantity and distribution in upper pressure hole 1 and pushing hole 2 are such as Shown in Fig. 2, the diameter in upper pressure hole 1 and pushing hole 2 is corresponding with rubber pad and the increase of metallic plate bond area to be increased;
(Two)According to pushing hole 1 and pushing the distribution in hole 2, the round steel 3 of respective numbers is selected, and steel seat 4 is fixed on circle One end of steel 3;
(Three)Rubber pad is placed on pressure testing machine 200, the round steel 3 and steel seat 4 coordinated with upper pressure hole 1 is placed in rubber pad Top, and push round steel 3 that hole 2 coordinates and steel seat 4 is placed in the lower section of rubber pad, adjust pressure testing machine, make pressure head and bottom After disk is contacted with steel seat 4 respectively, the load reading of pressure testing machine is adjusted to zero-bit;
(Four)The speed that pressure head moves downward adjusts after 10 ~ 20mm/min, starts pressure testing machine 200, and pressure head pushes, It presses round steel 3 and steel seat 4 on hole 1 to move downward in drive, the distance of upper layer metallic plate 100 and lower metal plate 101 is made to increase, Rubber layer 102 is stretched, until upper layer metallic plate 100 and lower metal plate 101 are detached from rubber layer 102 simultaneously, stops pushing Pressure head, and record the load reading of pressure testing machine 200;
(Five)By the quantity and diameter in upper pressure hole 1 and pushing hole 2, metallic plate is bonding with rubber layer when calculating test Area S, that is, metallic plate and the bond area S of rubber layer are equal to the bond area of upper layer metallic plate 100 and rubber layer 102 when testing Subtract the sum of the hole area in upper pressure hole 1 and pushing hole 2 in rubber pad.
(Six)The adhesive strength P, P=F/S of rubber layer and metallic plate is calculated.
The technical solution of the embodiment of the present invention is completely described above in association with attached drawing, it should be noted that described Embodiment be only the present invention a part of the embodiment.Based on the embodiments of the present invention, those of ordinary skill in the art exist The every other embodiment obtained under the premise of not making creative work, shall fall within the protection scope of the present invention.

Claims (10)

1. rubber pad rubber adhesive strength test method selects round rubber pad or polygon rubber pad to be tested, rubber pad In each layer metallic plate and the bond area of rubber layer be equal, rubber pad is horizontally disposed with, with vertical force-extension adjacent two layers Rubber layer between metallic plate, until rubber layer is detached from metallic plate, it is vertical when detection metallic plate is detached from rubber layer External force F and when test metallic plate and rubber layer bond area S, the ratio for calculating F and S is worth to the viscous of rubber layer and metallic plate Meet intensity P, it is characterised in that the adjacent two layers metallic plate is respectively upper layer metallic plate(100)With lower metal plate(101), It opens up and is vertically staggered and upper pressure hole that diameter is equal on the rubber pad(1)With pushing hole(2), the upper pressure hole (1)It is opened up from the top surface of rubber pad across upper layer metallic plate(100)To the top surface of lower metal plate (101), the pushing hole (2)It is opened up from the bottom surface of rubber pad across lower metal plate(101)To upper layer metallic plate(100)Bottom surface, upper pressure hole(1)With under Press hole(2)In be inserted into round steel(3), upper pressure hole is made under the action of vertical external force(1)In round steel(3)It moves downward, upper layer Metallic plate(100)With lower metal plate(101)Distance increases, and stretches upper layer metallic plate(100)With lower metal plate(101)Between Rubber layer(102), until upper layer metallic plate(100)And/or lower metal plate(101)With rubber layer(102)With detach.
2. rubber pad rubber adhesive strength test method according to claim 1, it is characterised in that above press hole(1)Hole face The sum of product and pushing hole(2)The sum of hole area be not less than the 1/15 of metallic plate and the bond area of rubber layer.
3. rubber pad rubber adhesive strength test method according to claim 2, it is characterised in that the upper pressure hole(1)With Push hole(2)Quantity it is equal, and upper pressure hole(1)With pushing hole(2)Uniformly isolation distribution on the same circumference, it is two adjacent Upper pressure hole(1)Between distribution one pushing hole(2).
4. rubber pad rubber adhesive strength test method according to claim 3, it is characterised in that the upper pressure hole(1) With pushing hole(2)The area of circumference where being distributed accounts for the 1/3 ~ 1/2 of metallic plate and the bond area of rubber layer.
5. rubber pad rubber adhesive strength test method according to claim 3, it is characterised in that above press hole(1)Diameter For 16 ~ 24mm, quantity is 4 ~ 8.
6. according to claim 3 to claim 5 any one of them rubber pad rubber adhesive strength test method, feature exists In the round steel(3)Length be 3 ~ 4 times of rubber mat thickness, round steel(3)One end and upper pressure hole(1)Or push hole(2)Between Gap coordinates.
7. rubber pad rubber adhesive strength test method according to claim 6, it is characterised in that be placed in the upper pressure Hole(1)In round steel(3)Pass through steel seat(4)Connection forms entirety, is placed in and pushes hole(2)In round steel(3)Also by steel seat(4) Connection forms whole, described steel seat(4)Horizontally disposed steel seat parallel with rubber pad, described(4)It is fixed on round steel(3)It is another One end, vertical force act on steel seat(4)On make pressure hole(1)In round steel(3)It moves downward.
8. rubber pad rubber adhesive strength test method according to claim 7, it is characterised in that pass through pressure testing machine Offer acts on steel seat(4)On vertical force, the rubber pad is set on pressure testing machine, upper pressure hole(1)In round steel (3)The steel seat of end(4)It is contacted with the pressure head of pressure testing machine, pushes hole(2)In round steel(3)The steel seat of end(4)With pressure The chassis of force tester contacts, and Opening pressure testing machine, pressure head moves downward, and pressure acts on steel seat(4)On make pressure hole(1) In round steel(3)It moves downward, upper layer metallic plate(100)With lower metal plate(101)Distance increases, when upper layer metallic plate (100)With lower metal plate(101)With rubber layer(102)When with being detached from, the load reading of pressure testing machine is metallic plate and rubber Vertical external force F when glue-line is detached from.
9. rubber pad rubber adhesive strength test method according to claim 8, it is characterised in that " when test metallic plate with The bond area S " of rubber layer refers to upper layer metallic plate(100)With rubber layer(102)Bond area subtract in rubber pad pressure Hole(1)With pushing hole(2)The sum of hole area.
10. the rubber pad rubber adhesive strength test method according to claim 8 or claim 9, it is characterised in that pressure When force tester is opened, the speed control that pressure head moves downward is in 10 ~ 20mm/min.
CN201610581146.9A 2016-07-21 2016-07-21 Rubber pad rubber adhesive strength test method Expired - Fee Related CN106290147B (en)