CN106040514A - Brushing method of chemical pump body paint - Google Patents
Brushing method of chemical pump body paint Download PDFInfo
- Publication number
- CN106040514A CN106040514A CN201610478603.1A CN201610478603A CN106040514A CN 106040514 A CN106040514 A CN 106040514A CN 201610478603 A CN201610478603 A CN 201610478603A CN 106040514 A CN106040514 A CN 106040514A
- Authority
- CN
- China
- Prior art keywords
- paint
- brushing
- chemical pump
- putty
- dry
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention relates to the technical field of pump valve manufacturing, in particular to a brushing method of chemical pump body paint. The brushing method comprises the following steps that through chemical pump surface pretreatment, rust removal and dirt and oil removal are carried out; then putty smearing is carried out; and after drying, three times of paint brushing are carried out, and then the paint is dried. The brushing method has the beneficial effects that the technological process is simple and convenient to operate; chemical pump paint brushing is carried out through the scientific and reasonable method; the fastness performance of the chemical pump surface paint is guaranteed, and the paint is not prone to falling off; and by means of chemical pump surface pretreatment, strong assistance of the paint is guaranteed, durability is high, and the paint is durable.
Description
Technical field
The present invention relates to pump valve preparing technical field, be specifically related to the brushing method of a kind of chemical pump pump housing paint.
Background technology
Chemical pump is the energy-saving pump of Joint National design, and pump performance, technology requirement, according to the property of international standard defined
Can be with size design, its advantage: complete series conservancy property is rationally distributed, user's range of choice width, " rear open type " structure, maintenance
Convenient, efficiency and suction are reached advanced world standards, and are widely used in industry, city water, draining, also can be used for farmland, orchard
Irrigation and drainage, other liquid being similar to clear water for conveying clear water or physics and chemical property are used, chemical pump when normally using, due to
The application of the pump housing is different, uses in touching some industries possessing corrosive nature meson, and therefore chemical pump is normally
Processing in, all can carry out paint on pump housing surface, not only ensure its corresponding aesthetic property, simultaneously can with anticorrosion,
Improve service life, but owing to chemical pump is in normal use, certain high heat fluid conveying can be related to, therefore surpass
The fluid of high heat can make the paint on chemical pump surface by great high temperature, it is easy to de-after causing certain paint to be heated
Fall, the most how to carry out the reasonable coating painted, it is to avoid it is the research topic that this area is necessary at present that paint high temperature comes off.
Summary of the invention:
The technical problem to be solved is to provide a kind of technological process simple, and effect is notable, method letter
The brushing method of single chemical pump pump housing paint.
The technical problem to be solved realizes by the following technical solutions:
The brushing method of a kind of chemical pump pump housing paint, it is characterised in that comprise the following steps:
1) chemical pump treating brushing paint carrying out surface rusty stain removing, sweep-out method uses sand paper to carry out detail sanding,
Until after surface is visible by naked eyes rusty stain, using air gun to be blown off by surface anvil cinder;
2), after using clear water hydro-peening clean on chemical pump surface after above-mentioned rust cleaning, the hot water being again with boiling carries out one
Secondary drip washing, after drip washing, uses rapidly hot-air blower, is done by surface moisture hot blow;This step is for by attachment on chemical pump surface
Major part oils and fats tentatively cleans;
3) select quick lime to be sprinkling upon chemical pump surface, after then adding water to watering can, be sprayed at chemical pump surface, the most quiet
After putting 5-7min, use clear water to rinse well, be then again with hot-air blower and dry up;
4) allotment powder of lacquer putty for use on, moves chemical pump to dust-free workshop, at one layer of powder of lacquer putty for use on of chemical pump surface brush, powder of lacquer putty for use on
THICKNESS CONTROL, between 0.5-1.5mm, then stands until powder of lacquer putty for use on forms putty layering after drying;
5) treating that the layering of above-mentioned putty is dried, using sand paper putty layering to be polished, until ensureing putty bisque
THICKNESS CONTROL is between 0.5-0.8mm;
6) chemical pump after above-mentioned steps 5 being processed moves to drying room, controls drying room temperature and is 45-48 DEG C, quiet to baking
25-28min;
7) chemical pump after above-mentioned baking is moved again to dust-free workshop, surface particles thing employing air gun is blown clean
After, carrying out painting for the first time brushing, the THICKNESS CONTROL of paint brushing is at 0.2-0.3mm;
8) after paint eighty per cant after above-mentioned brushing is dry, again carrying out second time and paint brushing, brushing paint is thick for the second time
Degree is 0.1-0.2mm;
9) after in above-mentioned steps 8 seventy percent is dry, carrying out third time and paint brushing, the thickness of third time paint brushing is 0.4-
0.5mm, after brushing terminates, after standing to sixty percent is dry, moves integrally chemical pump to drying room, and in control drying room, temperature is 38-
45 DEG C, baking until paint absolutely dry after,.
The powder of lacquer putty for use on used in above-mentioned steps 4 is oil putty;
The invention has the beneficial effects as follows: present invention process flow process is simple and convenient, carry out chemical industry by scientific and reasonable method
Pump paint brushing, it is ensured that the firm performance of chemical pump surface paint, difficult drop-off, by by chemical pump surface preparation, protect
The strength auxiliary of card paint, persistency is strong, durable in use.
Detailed description of the invention
For the technological means making the present invention realize, creation characteristic, reach purpose and be easy to understand with effect, below knot
Close specific embodiment, the present invention is expanded on further.
Embodiment 1
The brushing method of a kind of chemical pump pump housing paint, comprises the following steps:
1) chemical pump treating brushing paint carrying out surface rusty stain removing, sweep-out method uses sand paper to carry out detail sanding,
Until after surface is visible by naked eyes rusty stain, using air gun to be blown off by surface anvil cinder;
2), after using clear water hydro-peening clean on chemical pump surface after above-mentioned rust cleaning, the hot water being again with boiling carries out one
Secondary drip washing, after drip washing, uses rapidly hot-air blower, is done by surface moisture hot blow;This step is for by attachment on chemical pump surface
Major part oils and fats tentatively cleans;
3) select quick lime to be sprinkling upon chemical pump surface, after then adding water to watering can, be sprayed at chemical pump surface, the most quiet
After putting 5min, use clear water to rinse well, be then again with hot-air blower and dry up;
4) allotment powder of lacquer putty for use on, moves chemical pump to dust-free workshop, at one layer of powder of lacquer putty for use on of chemical pump surface brush, powder of lacquer putty for use on
THICKNESS CONTROL, between 0.5mm, then stands until powder of lacquer putty for use on forms putty layering after drying;
5) treating that the layering of above-mentioned putty is dried, using sand paper putty layering to be polished, until ensureing putty bisque
THICKNESS CONTROL is between 0.5mm;
6) chemical pump after above-mentioned steps 5 being processed moves to drying room, and controlling drying room temperature is 45 DEG C, quiet to baking
25min;
7) chemical pump after above-mentioned baking is moved again to dust-free workshop, surface particles thing employing air gun is blown clean
After, carrying out painting for the first time brushing, the THICKNESS CONTROL of paint brushing is at 0.2mm;
8) after paint eighty per cant after above-mentioned brushing is dry, again carrying out second time and paint brushing, brushing paint is thick for the second time
Degree is 0.1mm;
9) after in above-mentioned steps 8 seventy percent is dry, carrying out third time and paint brushing, the thickness of third time paint brushing is
0.4mm, after brushing terminates, after standing to sixty percent is dry, moves integrally chemical pump to drying room, and in control drying room, temperature is 38
DEG C, baking until paint absolutely dry after,.
Embodiment 2
The brushing method of a kind of chemical pump pump housing paint, comprises the following steps:
1) chemical pump treating brushing paint carrying out surface rusty stain removing, sweep-out method uses sand paper to carry out detail sanding,
Until after surface is visible by naked eyes rusty stain, using air gun to be blown off by surface anvil cinder;
2), after using clear water hydro-peening clean on chemical pump surface after above-mentioned rust cleaning, the hot water being again with boiling carries out one
Secondary drip washing, after drip washing, uses rapidly hot-air blower, is done by surface moisture hot blow;This step is for by attachment on chemical pump surface
Major part oils and fats tentatively cleans;
3) select quick lime to be sprinkling upon chemical pump surface, after then adding water to watering can, be sprayed at chemical pump surface, the most quiet
After putting 7min, use clear water to rinse well, be then again with hot-air blower and dry up;
4) allotment powder of lacquer putty for use on, moves chemical pump to dust-free workshop, at one layer of powder of lacquer putty for use on of chemical pump surface brush, powder of lacquer putty for use on
THICKNESS CONTROL, between 1.5mm, then stands until powder of lacquer putty for use on forms putty layering after drying;
5) treating that the layering of above-mentioned putty is dried, using sand paper putty layering to be polished, until ensureing putty bisque
THICKNESS CONTROL is between 0.8mm;
6) chemical pump after above-mentioned steps 5 being processed moves to drying room, and controlling drying room temperature is 48 DEG C, quiet to baking
28min;
7) chemical pump after above-mentioned baking is moved again to dust-free workshop, surface particles thing employing air gun is blown clean
After, carrying out painting for the first time brushing, the THICKNESS CONTROL of paint brushing is at 0.3mm;
8) after paint eighty per cant after above-mentioned brushing is dry, again carrying out second time and paint brushing, brushing paint is thick for the second time
Degree is 0.2mm;
9) after in above-mentioned steps 8 seventy percent is dry, carrying out third time and paint brushing, the thickness of third time paint brushing is
0.5mm, after brushing terminates, after standing to sixty percent is dry, moves integrally chemical pump to drying room, and in control drying room, temperature is 45
DEG C, baking until paint absolutely dry after,.
The ultimate principle of the present invention and principal character and advantages of the present invention have more than been shown and described.The technology of the industry
Personnel, it should be appreciated that the present invention is not restricted to the described embodiments, simply illustrating this described in above-described embodiment and description
The principle of invention, without departing from the spirit and scope of the present invention, the present invention also has various changes and modifications, and these become
Change and improvement both falls within scope of the claimed invention.Claimed scope by appending claims and
Equivalent defines.
Claims (2)
1. the brushing method of a chemical pump pump housing paint, it is characterised in that comprise the following steps:
1) chemical pump treating brushing paint carrying out surface rusty stain removing, sweep-out method uses sand paper to carry out detail sanding, until
After surface is visible by naked eyes rusty stain, air gun is used to be blown off by surface anvil cinder;
2), after using clear water hydro-peening clean on chemical pump surface after above-mentioned rust cleaning, the hot water being again with boiling once drenches
Wash, after drip washing, use rapidly hot-air blower, surface moisture hot blow is done;
3) select quick lime to be sprinkling upon chemical pump surface, after then adding water to watering can, be sprayed at chemical pump surface, then stand 5-
After 7min, use clear water to rinse well, be then again with hot-air blower and dry up;
4) allotment powder of lacquer putty for use on, moves chemical pump to dust-free workshop, at one layer of powder of lacquer putty for use on of chemical pump surface brush, the thickness of powder of lacquer putty for use on
Control between 0.5-1.5mm, then stand until powder of lacquer putty for use on forms putty layering after drying;
5) treating that the layering of above-mentioned putty is dried, using sand paper putty layering to be polished, until ensureing the thickness of putty bisque
Control between 0.5-0.8mm;
6) chemical pump after above-mentioned steps 5 being processed moves to drying room, controls drying room temperature and is 45-48 DEG C, quiet to toasting 25-
28min;
7) chemical pump after above-mentioned baking is moved again to dust-free workshop, after surface particles thing employing air gun is blown clean, enters
Row paint brushing for the first time, the THICKNESS CONTROL of paint brushing is at 0.2-0.3mm;
8) after paint eighty per cant after above-mentioned brushing is dry, again carrying out second time and paint brushing, brushing paint thickness is for the second time
0.1-0.2mm;
9) after in above-mentioned steps 8 seventy percent is dry, carrying out third time and paint brushing, the thickness of third time paint brushing is 0.4-
0.5mm, after brushing terminates, after standing to sixty percent is dry, moves integrally chemical pump to drying room, and in control drying room, temperature is 38-
45 DEG C, baking until paint absolutely dry after,.
The brushing method of a kind of chemical pump pump housing the most according to claim 1 paint, it is characterised in that: in above-mentioned steps 4
The powder of lacquer putty for use on used is oil putty.