CN105506287A - 南方稀土矿浸出母液沉淀法回收稀土的工艺 - Google Patents

南方稀土矿浸出母液沉淀法回收稀土的工艺 Download PDF

Info

Publication number
CN105506287A
CN105506287A CN201610020976.4A CN201610020976A CN105506287A CN 105506287 A CN105506287 A CN 105506287A CN 201610020976 A CN201610020976 A CN 201610020976A CN 105506287 A CN105506287 A CN 105506287A
Authority
CN
China
Prior art keywords
rare earth
mother liquor
filtrate
rare
precipitation
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201610020976.4A
Other languages
English (en)
Other versions
CN105506287B (zh
Inventor
孙东江
王志勇
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Ganzhou rare earth mining technology service Co., Ltd.
Original Assignee
Jin Yi Mining Industry Co Ltd Of Longnan County
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jin Yi Mining Industry Co Ltd Of Longnan County filed Critical Jin Yi Mining Industry Co Ltd Of Longnan County
Priority to CN201610020976.4A priority Critical patent/CN105506287B/zh
Publication of CN105506287A publication Critical patent/CN105506287A/zh
Application granted granted Critical
Publication of CN105506287B publication Critical patent/CN105506287B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

一种南方稀土矿浸出母液沉淀法回收稀土的工艺,其步骤是,用泵将所收集的浸出稀土矿山母液打入搅拌桶中,加入氧化镁,调整pH值,混合沉淀浆水流入澄清池澄清,澄清后将上清液排至配液池,将沉淀物过滤,之后滤料加入清水调浆,然后加入酸溶解,再用板框压滤,滤液进入储液池,用NaOH溶液调pH值,再用板框压滤机过滤,滤液转入沉淀桶,在搅拌状态下用Na2CO3进行稀土沉淀,过滤,滤渣即为稀土碳酸盐供稀土冶炼厂分离。本发明能避免现有技术中的氨氮废水对环境的影响,特别是对低品位矿山、低浓度母液更是解决了回收率低、生产成本高的问题,本工艺稀土的回收率≧95%,为未来低品位稀土矿山的开采寻找到了一条新的生产工艺。

Description

南方稀土矿浸出母液沉淀法回收稀土的工艺
技术领域
本发明涉及一种南方稀土矿浸出母液沉淀法回收稀土的工艺。
背景技术
南方离子吸附型稀土矿又称风化壳淋积型稀土矿(简称南方稀土矿),20世纪60年代末在江西省龙南发现,尔后相继在福建、湖南、广东、广西等地区均有发现。经几十年的研究,查明该类型矿分布地面广、储量大、放射性低、开采容易、提取稀土工艺简单、产品质量好。
南方稀土矿的开采目前都在寻找一种相对友好的开采方式,在浸矿剂方面正由硫铵向镁盐、钠盐方向转换,目前已取得了一定的进展,如何利用一种新的沉淀模式来配套是一个新的问题。
发明内容
本发明的目的就是提供一种稀土回收率高、生产成本低,能减少环境污染的南方稀土矿浸出母液沉淀法回收稀土的工艺。
本发明的南方稀土矿浸出母液沉淀法回收稀土的工艺,包括以下步骤:
1、母液收集:将浸出稀土矿山母液引入母液池备用;
2、氧化镁准备:工业级、85%的氧化镁粉末;
3、氧化镁沉淀富集稀土:用水泵将所收集的浸出稀土矿山母液打入带有搅拌装置的搅拌桶中,加入氧化镁,调整pH=6.5~7,混合沉淀浆水通过溢流管流入澄清池澄清;
4、稀土沉淀物过滤:澄清后将上清液排至配液池,将沉淀物过滤,滤液排弃至配液池;
5、滤料溶解:将滤料转入PP材质的搅拌桶中加入清水调浆,然后缓慢加入酸溶解,维持溶解过程pH=3~3.5,待滤料中的氢氧化稀土溶解后,用板框压滤,滤液进入储液池备用,滤渣用50%浓度的硫酸溶解后作为浸矿剂使用;
6、稀土除杂:将滤料溶解所得滤液转入另一个PP材质的搅拌桶,用5%的NaOH溶液调pH=5.2~5.8,搅拌后用板框压滤机过滤,滤液转入沉淀桶,滤渣存放回收三氧化铝;
7、稀土沉淀:将除杂后转入沉淀桶中的滤液在搅拌状态下用Na2CO3调pH=6.7~7进行稀土沉淀,之后用板框过滤机过滤,滤液进入配浸矿剂池作循环浸矿使用,滤渣即为稀土碳酸盐供稀土冶炼厂分离。
本发明的南方稀土矿浸出母液沉淀法回收稀土的工艺,能避免现有技术中的氨氮废水对环境的影响,特别是对低品位矿山、低浓度母液更是解决了回收率低、生产成本高的问题,本工艺稀土的回收率≧95%,为未来低品位稀土矿山的开采寻找到了一条新的生产工艺。
具体实施方式
一种南方稀土矿浸出母液沉淀法回收稀土的工艺,以日处理400m3浓度为0.3g/L的稀土母液为例:
具体步骤:
1、母液收集:将400m3浸出稀土矿山母液引入400m3母液池备用,测试pH=4.5;
2、氧化镁(工业级、85%MgO)准备:在一带有搅拌器的20m3的搅拌桶上方设立的2m3料仓中投入100kg氧化镁粉末;
3、氧化镁沉淀富集稀土:用水泵把步骤1收集的母液打入步骤2搅拌桶中,开启搅拌,启动自动给料机给料,边打入母液边加氧化镁,混合沉淀浆水通过溢流管流入澄清池,待400m3母液全部中和沉淀完毕进入澄清池后,测试上清液pH值,如果pH<6.5则通过搅拌桶补加氧化镁调浆水使上清液pH达到6.5~7即可,澄清1小时后,放出上清液至浸矿剂配液池;
4、稀土沉淀物过滤:将步骤3放完上清液的底渣用离心泵打入板框压滤机过滤,滤液通过PVC管道引入浸矿剂配液池,滤渣收集备用;
5、滤料溶解:将步骤4所产生的滤渣转入一10m3PP材质的搅拌桶中,加同体积的水调浆,然后缓慢加入1:1盐酸溶解,反应终点以pH=3稳定半小时为准,然后通过板框压滤机压滤,滤液转入一个20m3PP材质的搅拌桶,滤渣堆存;
6、稀土除杂:将步骤5产生稀土母液在20m3PP材质桶中搅拌,以配好的5%的NaOH溶液为中和液调整稀土母液pH=5.4,然后静置1小时,放出上清液至一20m3PP材质搅拌桶中,底部沉淀渣浆通过板框压滤机压滤,滤液并入存放上清液的搅拌桶中,滤液堆存待处理;
7、稀土沉淀:将步骤6操作产生的稀土母液取样测试稀土浓度,在搅拌的条件下,加入母液中稀土总量的1.3倍(重量比)的固体碳酸钠进行稀土沉淀,加完碳酸钠后测试母液pH值,如果pH<6.7则需补加少量碳酸钠直至母液pH达到6.7~7为沉淀终点,然后经过板框压滤机过滤,滤液通过管道导入浸矿剂配液池,滤渣即为稀土碳酸盐供稀土冶炼厂分离。

Claims (1)

1.一种南方稀土矿浸出母液沉淀法回收稀土的工艺,其特征在于:它包括以下步骤:
(1)、母液收集:将浸出稀土矿山母液引入母液池备用;
(2)、氧化镁准备:工业级、85%的氧化镁粉末;
(3)、氧化镁沉淀富集稀土:用水泵将所收集的浸出稀土矿山母液打入带有搅拌装置的搅拌桶中,加入氧化镁,调整pH=6.5~7,混合沉淀浆水通过溢流管流入澄清池澄清;
(4)、稀土沉淀物过滤:澄清后将上清液排至配液池,将沉淀物过滤,滤液排弃至配液池;
(5)、滤料溶解:将滤料转入PP材质的搅拌桶中加入清水调浆,然后缓慢加入酸溶解,维持溶解过程pH=3~3.5,待滤料中的氢氧化稀土溶解后,用板框压滤,滤液进入储液池备用;
(6)、稀土除杂:将滤料溶解所得滤液转入另一个PP材质的搅拌桶,用5%的NaOH溶液调pH=5.2~5.8,搅拌后用板框压滤机过滤,滤液转入沉淀桶;
(7)、稀土沉淀:将除杂后转入沉淀桶中的滤液在搅拌状态下用Na2CO3调pH=6.7~7进行稀土沉淀,之后用板框过滤机过滤,滤渣即为稀土碳酸盐。
CN201610020976.4A 2016-01-13 2016-01-13 南方稀土矿浸出母液沉淀法回收稀土的工艺 Active CN105506287B (zh)