CN105000868A - 一种超低磨耗的瓷球及其制备方法 - Google Patents

一种超低磨耗的瓷球及其制备方法 Download PDF

Info

Publication number
CN105000868A
CN105000868A CN201510298749.3A CN201510298749A CN105000868A CN 105000868 A CN105000868 A CN 105000868A CN 201510298749 A CN201510298749 A CN 201510298749A CN 105000868 A CN105000868 A CN 105000868A
Authority
CN
China
Prior art keywords
porcelain ball
preparation
abrasion
ultralow
ball
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201510298749.3A
Other languages
English (en)
Other versions
CN105000868B (zh
Inventor
詹晔
罗金球
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kweiyang White Clouds Cloud And Mist Bauxite Calcination Process Factory
Original Assignee
Kweiyang White Clouds Cloud And Mist Bauxite Calcination Process Factory
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kweiyang White Clouds Cloud And Mist Bauxite Calcination Process Factory filed Critical Kweiyang White Clouds Cloud And Mist Bauxite Calcination Process Factory
Priority to CN201510298749.3A priority Critical patent/CN105000868B/zh
Publication of CN105000868A publication Critical patent/CN105000868A/zh
Application granted granted Critical
Publication of CN105000868B publication Critical patent/CN105000868B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种超低磨耗的瓷球及其制备方法,其制造原料来源于天然铝矾土,其主要化学成为Al2O3含量为72-83%,SiO2含量为22-15%,经混合研磨、成型、高温烧成,制得高强度,高密度(3.25g/cm3),超硬度(莫氏8-9级),超低磨耗(≤.06g/kg·h)的瓷球产品。本发明旨在简化传统工艺程序,去掉湿式陈腐,雾化干燥、破碎等工序,取得“均质化”的超微细粉,高温烧成促进“固相反应”,避免低温液相形成“固熔体”,让主晶相“刚玉一莫来石”结晶发育完全。本发明制造的瓷球,大大地提高了其性价比,具有质的飞跃。在建陶、特陶、日用陶、耐火材料、医药化工,非金属矿等行业中有着广泛应用前途。

Description

一种超低磨耗的瓷球及其制备方法
技术领域
本发明涉及非金属研磨介质技术领域,具体涉及一种超低磨耗的陶瓷球及其制备方法。
背景技术
传统生产的陶瓷球,无论产品品质或生产工艺都存在有明显的缺陷和弊端,同国外产品相比较,在质量和技术层面上差距很大。
1、传统的陶瓷工艺法生产陶瓷球,其工序繁复,厂房占地面大,设备多,产能低、能耗高。
2、传统陶瓷工艺法能生产优质的瓷器类产品,但不完全适应超低磨耗的瓷球生产,因为瓷球不是瓷器,前者是后者生产工艺装备中的|“工具”—研磨介质,所追求的终极目标是超低磨耗,以及被研磨的物料对产品不能产生质的影响。因此,传统的陶瓷工艺法,在瓷球生产工艺中,只能借鉴,不能完全套用。
发明内容
本发明的目的在于提供一种超低磨耗的瓷球及其制备方法,以克服传统陶瓷工艺法的不足。
本发明的一种超低磨耗的瓷球是这样的,其理化指标:Al2O3含量71-82%,SiO2含量26-15%,常温耐压强度≥180MPa,密度≥3.25g/cm3,莫氏硬度为8-9级,磨耗≤0.06g/kg·h。其采用天然铝矾土原料经混合研磨、成型、高温烧成;所述天然铝矾土化学成份指标为:Ae2O372-85%,SiO12-25%, Fe2O3<1.5%,熔融指数<1.8。
这种超低磨耗的瓷球的制备方法是这样的:采用天然铝矾土为原料,按以下步骤制备:
(1)全粉料制备:原料经混合研磨,细度控制600目,通过量不低于98%;
(2)物料在研磨前后两次除铁,自动除铁机磁强在8000-12000高斯;
(3)泥料制备:将除铁后的全粉料加结合剂硅溶胶溶液,强力搅拌混练15-30分钟,泥料水份控制在6.5-9%;
(4)将配好的泥料静放焖料4-8小时,让泥料结合剂充分浸润,排除气体;
(5)成型:焖好的泥料经容量加料,金属钢模具等静压压制成型,压力不低于100Mpa,自动脱模得到半成品瓷球;
(6)干燥:成型的瓷球坯体剔除不合格品,送入隧道干燥器,干燥温度控制在110-180℃,干燥时间16-24小时,球坯残余水份小于1.0%;
(7)烧成:干燥完后的球坯,拣选后装入匣缽,入窑码垛并按烧成曲线烧制;
(8)烧制的成品瓷球,取样检测。
其中,步骤(3)中所述硅溶胶溶液浓度为1%-5%。步骤(5)中成型的半成品瓷球干容重控制在2.75-2.8g/cm3。步骤(7)中所述烧成曲线如下:
升温阶段:常温1650℃,48-58小时;
保温阶段:1640℃±10℃,24-32小时;
冷却阶段:自然冷却,不鼓风,控制烟道闸板的开启度;在止火温度-1350℃,可急冷;1300℃以后,缓慢自然冷却,以免冷却收缩应力产生看不见的裂纹。
本发明相比现有技术,具有如下优点:
1、与现有的普通瓷球相比较,简化了生产工序,精简了设备设施,减少了厂房及厂房占地面积,在相同产量规模的条件下,装机容量减少30%,建筑面积减少20%,占地面积减少30%,岗位用工减少25%,显然减少了投资数额。
2、与现有的普通瓷球相比较,其产品质量耐磨性提高5倍,研磨效率提高20-40%,磨机的有效率提高15-25%,使用综合成本降低,就用户而言,提高了生产效率,降低了生产成本和资金流通量。
3、与现有的普通瓷球相比较,其产品质量的提高,其销售价格提高1.5-2.5倍,利润提高2-3倍。就经济效益和社会效益而言,节约了矿产资源、人力资源,降低了能源消耗,水资源消耗,减少废气的排量,有利于环境的保护。企业本身获得最大的利益,有利于降低投资风险以及日后的发展。
具体实施方式,
下面结合实施例对本发明作进一步的详细说明。
实施例1:
超低磨耗瓷球的理化指标:Al2O3含量71-82%,SiO2含量26-15%,常温耐压强度≥180MPa,密度≥3.25g/cm3,硬度(莫氏)8-9级,磨耗≤0.06g/kg·h。
制备方法:
采用原料为天然铝矾土,其化学成份指标为:Ae2O372-85%,SiO212-25%, Fe2O3<1.5%,熔融指数<1.8。
全粉料制备,原料经混合研磨,细度控制600目,通过量不低于98%。
物料在研磨前后两次除铁,自动除铁机磁强在8000-12000高斯。
泥料制备,重量配料,百分之百的粉料,外加结合剂,硅溶胶溶液(浓度1%-5%),强力搅拌混练15-30分钟,泥料水份控制在6.5-9%。
配好的泥料,静放焖料4-8小时,让泥料结合剂充分浸润,排除气体。
成型,等静压压制成型,压力不低于100Mpa,焖好的泥料经容量加料,金属钢模具,自动脱模,半成品瓷球干容重(密度)控制在2.75-2.8g/cm3
干燥,成型的瓷球坯体剔除不合格品,送入隧道干燥器,干燥温度控制在110-180℃,干燥时间16-24小时,球坯残余水份小于1.0%。
烧成,高温节能环保型轮式窑,刚玉一莫来石匣缽。干燥完后的球坯,拣选后装入匣缽,入窑码垛。按以下烧成曲线烧制。
升温阶段:常温1650℃,  48-58小时。
保温阶段:1640℃±10℃,24-32小时。
冷却阶段:自然冷却,不鼓风,控制烟道闸板的开启度,在止火温度-1350℃,可急冷。1300℃以后,应缓慢自然冷却,以免冷却收缩应力产生看不见的裂纹。
烧制的成品瓷球,取样检测,强度、密度、磨耗等关键指标,是本发明的特征体现。
瓷球的特征体现超低磨耗原于材质具有的高硬度和很好的耐磨性能。归根到底,是瓷球生产工艺流程终结时,瓷球完成了一系列的物理化学变化,演变成我们希望得到的“刚玉一莫来石”(Al2O3-3Al2O3. 2SiO2)晶相结构的新物体。在自然界中,“刚玉一莫来石”晶体的硬度仅次于最硬的金刚石。
本发明纯属适用型新型产品新技术类别,极易形成工业企业生产,产品可取代普通瓷球,推向市场有着广淍阔的前景。
1、原材料易得。天然铝矾土,在我国资源丰富,遍布南北数省,且价格低廉。
2、销售市场广阔。我国陶瓷工业发达,瓷球的需求量大,还可以出口,走向国际市场。
3、容易形成生产能力。本发明的工业应用,建设生产线,无需特大的资金投入。如产量在5000吨/年左右吨规模投资约在1500元—1800元;如产量在10000吨/年左右,吨规模投资约在2000-3000万元。生产工艺装备技术容易控制,维修方便,配件易得。消化掌握本发明技术,无需高学历的专业人才,岗位用工人力资源不会紧缺。
当然,以上只是本发明的具体应用范例,本发明还有其他的实施方式,凡采用等同替换或等效变换形成的技术方案,均落在本发明所要求的保护范围之内。

Claims (6)

1.一种超低磨耗的瓷球,其特征在于:其理化指标:Al2O3含量71-82%,SiO2含量26-15%,常温耐压强度≥180MPa,密度≥3.25g/cm3,莫氏硬度为8-9级,磨耗≤0.06g/kg·h。
2.根据权利要求1所述的超低磨耗的瓷球,其特征在于:其采用天然铝矾土原料经混合研磨、成型、高温烧成;所述天然铝矾土化学成份指标为:Ae2O372-85%,SiO212-25%, Fe2O3<1.5%,熔融指数<1.8。
3.一种如权利要求1所述的超低磨耗的瓷球的制备方法,其特征在于:采用天然铝矾土为原料,按以下步骤制备:
(1)全粉料制备:原料经混合研磨,细度控制600目,通过量不低于98%;
(2)物料在研磨前后两次除铁,自动除铁机磁强在8000-12000高斯;
(3)泥料制备:将除铁后的全粉料加结合剂硅溶胶溶液,强力搅拌混练15-30分钟,泥料水份控制在6.5-9%;
(4)将配好的泥料静放焖料4-8小时,让泥料结合剂充分浸润,排除气体;
(5)成型:焖好的泥料经容量加料,金属钢模具等静压压制成型,压力不低于100Mpa,自动脱模得到半成品瓷球;
(6)干燥:成型的瓷球坯体剔除不合格品,送入隧道干燥器,干燥温度控制在110-180℃,干燥时间16-24小时,球坯残余水份小于1.0%;
(7)烧成:干燥完后的球坯,拣选后装入匣缽,入窑码垛并按烧成曲线烧制;
(8)烧制的成品瓷球,取样检测。
4.据权利要求3所述的超低磨耗的瓷球的制备方法,其特征在于:步骤(3)中所述硅溶胶溶液浓度为1%-5%。
5.据权利要求3所述的超低磨耗的瓷球的制备方法,其特征在于:步骤(5)中成型的半成品瓷球干容重控制在2.75-2.8g/cm3
6.根据权利要求3所述的超低磨耗的瓷球的制备方法,其特征在于:步骤(7)中所述烧成曲线如下:
升温阶段:常温1650℃,48-58小时;
保温阶段:1640℃±10℃,24-32小时;
冷却阶段:自然冷却,不鼓风,控制烟道闸板的开启度;在止火温度-1350℃,可急冷;1300℃以后,缓慢自然冷却,以免冷却收缩应力产生看不见的裂纹。
CN201510298749.3A 2015-06-03 2015-06-03 一种超低磨耗的瓷球及其制备方法 Expired - Fee Related CN105000868B (zh)