CN104005268A - 一种抗菌防潮高品质水松纸原纸及其制备方法 - Google Patents

一种抗菌防潮高品质水松纸原纸及其制备方法 Download PDF

Info

Publication number
CN104005268A
CN104005268A CN201410237004.1A CN201410237004A CN104005268A CN 104005268 A CN104005268 A CN 104005268A CN 201410237004 A CN201410237004 A CN 201410237004A CN 104005268 A CN104005268 A CN 104005268A
Authority
CN
China
Prior art keywords
parts
water
paper
quality
add
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201410237004.1A
Other languages
English (en)
Other versions
CN104005268B (zh
Inventor
杜威
雍宗友
牛和建
郭杰
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Chuzhou Cigarette Materials Factory
Original Assignee
Chuzhou Cigarette Materials Factory
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Chuzhou Cigarette Materials Factory filed Critical Chuzhou Cigarette Materials Factory
Priority to CN201410237004.1A priority Critical patent/CN104005268B/zh
Publication of CN104005268A publication Critical patent/CN104005268A/zh
Application granted granted Critical
Publication of CN104005268B publication Critical patent/CN104005268B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种抗菌防潮高品质水松纸原纸,其特征在于,由下列重量份的原料制备制成:硅酸钙1-2、硅胶干燥剂1-2、山梨酸0.8-1、甘蔗渣浆34-39、松木浆49-53、过氧化钙1-2、淀粉1.5-2、瓜尔胶2-3、白胶香0.8-1、烷基烯酮二聚体0.7-0.9、山梨糖醇0.5-0.7、山葵3-4、柚子皮3-5、碳酸钙2-3、助剂1-2、水适量;本发明添加硅胶干燥剂,安全无毒,能够起到防潮作用,添加山葵,充分利用植物的特点,具有抗菌以及净化烟气的作用,添加助剂,改善了烟气呛鼻的气味,使得制成的水松纸纤维分布均匀,透气度好,强度大,易于印刷,品质高。

Description

一种抗菌防潮高品质水松纸原纸及其制备方法
技术领域
本发明涉及香烟技术领域,特别是一种抗菌防潮高品质水松纸原纸及其制备方法。
背景技术
无论是在社交场合给人敬烟或接受敬烟,还是自己吸烟,一般都是用拇指和食指捏住卷烟水松纸将烟支取出,然后送到嘴中,而手指由于种种因素往往沾有大量的病菌或脏物;再者,卷烟水松纸的制造、印刷、储运以及卷烟的生产所处环境都不是无菌的,因而,水松纸会不可避免地沾染上环境中的微生物,包括许多致病菌、霉菌。这样,卷烟水松纸便成了病菌的传播媒介,导致“病从口入”,使人体健康因吸烟而受到威胁。
发明内容
本发明的目的是提供一种抗菌防潮高品质水松纸原纸及其制备方法。
为了实现本发明的目的,本发明通过以下方案实施:
一种抗菌防潮高品质水松纸原纸,由下列重量份的原料制备制成:硅酸钙1-2、硅胶干燥剂1-2、山梨酸0.8-1、甘蔗渣浆34-39、松木浆49-53、过氧化钙1-2、淀粉1.5-2、瓜尔胶2-3、白胶香0.8-1、烷基烯酮二聚体0.7-0.9、山梨糖醇0.5-0.7、山葵3-4、柚子皮3-5、碳酸钙2-3、助剂1-2、水适量;
所述助剂由以下重量份的原料制成:柠檬冻干粉4-5、小黄瓜冻干粉2-4、粉碎柠檬草2-4、粗孔硅胶2-3、白土3-5、迷迭香精油1-2、黄原胶 0.8-1、水适量;制备方法是将柠檬冻干粉、小黄瓜冻干粉、粉碎柠檬草、粗孔硅胶、白土混合粉碎成60-80目的粉末,然后加入迷迭香精油、少量水进行研磨,研磨20-30分钟后加水稀释成固含量为10-15%的溶液,最后加入黄原胶搅拌均匀,得到悬浊液即得。
本发明所述一种抗菌防潮高品质水松纸原纸,由以下具体步骤制成:
(1)将山葵、柚子皮加入2-3倍的水进行煎煮,过滤,滤液待用,取滤渣加入16倍重量份的浓度为1%的氢氧化钠浸泡8小时,加热至沸腾,小火蒸煮 2小时,然后水洗不溶物至无色,再用浓度为5%的盐酸和浓度为 4%的碳酸钠水溶液反复洗涤,直至不溶物的 pH 值为 7±0.2,然后干燥不溶物,即得植物纤维。
(2)将植物纤维、甘蔗渣浆、松木浆放入水力碎浆机碎解,再经打浆机,打浆浓度控制在3.5-4.5%,叩解度在66~740SR,制得浆料;
(3)将过氧化钙、硅酸钙、硅胶干燥剂混合均匀,研磨成40-60目的粉末,加入淀粉,搅拌25-30分钟制成混合料,然后在50-60℃烘干1-1.5小时待用;
(4)将混合料加入浆料中,加入除助剂以外的其余剩余成分,搅拌均匀,加入步骤(1)中滤液以及适量的水调浆至固含量为2.7-3.5%,加热至65-72℃,将调好的浆料经网部及压榨部脱水成形,湿纸页进入前干阶段,在表面均匀涂刷助剂;
(5)在0.05-0.08Mpa的真空条件下对成型后的湿纸进行抽吸脱水,然后电热鼓风干燥5-6min,最后在光机上进行压光,取出后即得水松纸原纸。
本发明的有益效果是:本发明添加硅胶干燥剂,安全无毒,能够起到防潮作用,添加山葵,充分利用植物的特点,具有抗菌以及净化烟气的作用,添加助剂,改善了烟气呛鼻的气味,使得制成的水松纸纤维分布均匀,透气度好,强度大,易于印刷,品质高。
具体实施方案
下面通过具体实例对本发明进行详细说明。
一种抗菌防潮高品质水松纸原纸,由下列重量份(公斤)的原料制备制成:硅酸钙1、硅胶干燥剂1、山梨酸0.8、甘蔗渣浆34、松木浆49、过氧化钙1、淀粉1.5、瓜尔胶2、白胶香0.8、烷基烯酮二聚体0.7、山梨糖醇0.5、山葵3、柚子皮3、碳酸钙2、助剂1、水适量;
所述助剂由以下重量份(公斤)的原料制成:柠檬冻干粉4、小黄瓜冻干粉2、粉碎柠檬草2、粗孔硅胶2、白土3、迷迭香精油1、黄原胶 0.8、水适量;制备方法是将柠檬冻干粉、小黄瓜冻干粉、粉碎柠檬草、粗孔硅胶、白土混合粉碎成60-80目的粉末,然后加入迷迭香精油、少量水进行研磨,研磨20-30分钟后加水稀释成固含量为10-15%的溶液,最后加入黄原胶搅拌均匀,得到悬浊液即得。
本发明所述一种抗菌防潮高品质水松纸原纸,由以下具体步骤制成:
(1)将山葵、柚子皮加入2-3倍的水进行煎煮,过滤,滤液待用,取滤渣加入16倍重量份的浓度为1%的氢氧化钠浸泡8小时,加热至沸腾,小火蒸煮 2小时,然后水洗不溶物至无色,再用浓度为5%的盐酸和浓度为 4%的碳酸钠水溶液反复洗涤,直至不溶物的 pH 值为 7±0.2,然后干燥不溶物,即得植物纤维。
(2)将植物纤维、甘蔗渣浆、松木浆放入水力碎浆机碎解,再经打浆机,打浆浓度控制在3.5-4.5%,叩解度在66~740SR,制得浆料;
(3)将过氧化钙、硅酸钙、硅胶干燥剂混合均匀,研磨成40-60目的粉末,加入淀粉,搅拌25-30分钟制成混合料,然后在50-60℃烘干1-1.5小时待用;
(4)将混合料加入浆料中,加入除助剂以外的其余剩余成分,搅拌均匀,加入步骤(1)中滤液以及适量的水调浆至固含量为2.7-3.5%,加热至65-72℃,将调好的浆料经网部及压榨部脱水成形,湿纸页进入前干阶段,在表面均匀涂刷助剂;
(5)在0.05-0.08Mpa的真空条件下对成型后的湿纸进行抽吸脱水,然后电热鼓风干燥5-6min,最后在光机上进行压光,取出后即得水松纸原纸。
经检测,本发明制得的水松纸原纸的纵向抗张强度为1.67KN/m,透气度为69CU。

Claims (2)

1.一种抗菌防潮高品质水松纸原纸,其特征在于,由下列重量份的原料制备制成:硅酸钙1-2、硅胶干燥剂1-2、山梨酸0.8-1、甘蔗渣浆34-39、松木浆49-53、过氧化钙1-2、淀粉1.5-2、瓜尔胶2-3、白胶香0.8-1、烷基烯酮二聚体0.7-0.9、山梨糖醇0.5-0.7、山葵3-4、柚子皮3-5、碳酸钙2-3、助剂1-2、水适量;
所述助剂由以下重量份的原料制成:柠檬冻干粉4-5、小黄瓜冻干粉2-4、粉碎柠檬草2-4、粗孔硅胶2-3、白土3-5、迷迭香精油1-2、黄原胶 0.8-1、水适量;制备方法是将柠檬冻干粉、小黄瓜冻干粉、粉碎柠檬草、粗孔硅胶、白土混合粉碎成60-80目的粉末,然后加入迷迭香精油、少量水进行研磨,研磨20-30分钟后加水稀释成固含量为10-15%的溶液,最后加入黄原胶搅拌均匀,得到悬浊液即得。
2.根据权利要求1所述一种抗菌防潮高品质水松纸原纸,其特征在于,由以下具体步骤制成:
(1)将山葵、柚子皮加入2-3倍的水进行煎煮,过滤,滤液待用,取滤渣加入16倍重量份的浓度为1%的氢氧化钠浸泡8小时,加热至沸腾,小火蒸煮 2小时,然后水洗不溶物至无色,再用浓度为5%的盐酸和浓度为 4%的碳酸钠水溶液反复洗涤,直至不溶物的 pH 值为 7±0.2,然后干燥不溶物,即得植物纤维;
(2)将植物纤维、甘蔗渣浆、松木浆放入水力碎浆机碎解,再经打浆机,打浆浓度控制在3.5-4.5%,叩解度在66~740SR,制得浆料;
(3)将过氧化钙、硅酸钙、硅胶干燥剂混合均匀,研磨成40-60目的粉末,加入淀粉,搅拌25-30分钟制成混合料,然后在50-60℃烘干1-1.5小时待用;
(4)将混合料加入浆料中,加入除助剂以外的其余剩余成分,搅拌均匀,加入步骤(1)中滤液以及适量的水调浆至固含量为2.7-3.5%,加热至65-72℃,将调好的浆料经网部及压榨部脱水成形,湿纸页进入前干阶段,在表面均匀涂刷助剂;
(5)在0.05-0.08Mpa的真空条件下对成型后的湿纸进行抽吸脱水,然后电热鼓风干燥5-6min,最后在光机上进行压光,取出后即得水松纸原纸。
CN201410237004.1A 2014-05-30 2014-05-30 一种抗菌防潮高品质水松纸原纸及其制备方法 Active CN104005268B (zh)