CN103952774A - 一种含纳米TiO2桑蚕丝的制备方法 - Google Patents
一种含纳米TiO2桑蚕丝的制备方法 Download PDFInfo
- Publication number
- CN103952774A CN103952774A CN201410167522.0A CN201410167522A CN103952774A CN 103952774 A CN103952774 A CN 103952774A CN 201410167522 A CN201410167522 A CN 201410167522A CN 103952774 A CN103952774 A CN 103952774A
- Authority
- CN
- China
- Prior art keywords
- tio
- silk
- mulberry
- nano
- mulberry silk
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
本发明公开了一种含纳米TiO2桑蚕丝的制备方法,首先将纳米TiO2配置成浓度为100~150mg/L的添加剂溶液,再将溶液按照100kg桑叶添加1.0L溶液的使用剂量喷洒桑叶,晾干后对家蚕五龄第3天的家蚕添食到上蔟,生产的桑蚕丝中Ti元素的含量为440±21~500±25ng/g,丝经水洗50次,Ti元素的含量为418±19~465±30ng/g,表明纳米TiO2和丝蛋白有很好的结合,耐水洗,稳定性高。本发明不采用化学试剂实现了含有纳米TiO2的制备,为桑蚕丝改性研究提供了新的研究思路。所公开的方法实用性强、操作方便、成本低、易于推广应用,不会对环境产生影响。
Description
技术领域
本发明涉及一种纳米粒子改性桑蚕丝的制备方法,具体涉及一种含纳米TiO2桑蚕丝的制备方法。
背景技术
桑蚕又称家蚕(Bombyx mori),是重要的绢丝昆虫,生产的桑蚕丝由于具有良好吸湿、保暖性能和具有穿着舒适性,柔软、光滑和弹性强的优点。丝织织物具有光泽柔和、雍容华丽、手感滑爽,还具有其他化学纤维无法比拟的天然保健功能,被誉为“纤维皇后”。
但是桑蚕丝长期暴露于太阳光线下,会泛黄和老化,抗皱性能较差,容易滋生病原微生物。针对桑蚕丝以上的缺点进行改良,是近年来研究桑蚕丝改性的热点。
纳米氧化物由于其独特的小尺寸效应、表面效应、量子尺寸效应及宏观量子隧道效应而具有优于常规粒子的热、磁、光敏感特性以及表面稳定性,从而应用于各个方面,如工业中的涂料和颜料领域,日常生活中的陶瓷、防晒化妆品及食品领域,环境治理中用于空气净化、污水处理和抗菌除毒领域。在纳米抗菌材料中抗菌剂以纳米尺寸分散,具有高比表面积和高反应活性,抗菌材料整体的抗菌效果较传统抗菌剂有显著提高,更能显著的抑制细菌、真菌等微生物的生长和繁殖,同时纳米氧化物高效的催化性能又可以促使化学毒剂降解。
现有技术中,以桑蚕丝为对象,采用化学试剂二羟甲基二羟基环乙烯脲树脂对桑蚕丝表面进行改性,可以将纳米TiO2结合到蚕丝的表面;用化学试剂钛酸四丁酯还可以把少量纳米TiO2结合到纤维内部微小的空隙中;但由于采用了化学试剂,在一定程度上改变了桑蚕丝的天然属性,改性后的桑蚕丝不能得到消费者的认可,并且由此方法得到的材料中,纳米TiO2与桑蚕丝附着力差。所以,很有必要研发一种新型的天然的方法制备出稳定的含纳米TiO2的桑蚕丝。
发明内容
本发明的目的是提供一种含纳米TiO2桑蚕丝的制备方法,以提高桑蚕丝的性能。
为达到上述发明目的,本发明采用的技术方案是:一种含纳米TiO2桑蚕丝的制备方法,包括如下步骤:
(1) 添加剂溶液的配制:将纳米TiO2与水进行混合后配制成浓度为100~150mg/L的添加剂溶液;
(2) 添食家蚕:将步骤(1)中制备的添加剂溶液按照100kg桑叶添加1L溶液剂量喷洒适熟叶,待适熟叶晾干后,对发育到五龄第3天的家蚕连续添食至上蔟;
(3) 缫丝:对步骤(2)中生长至上蔟阶段的家蚕蚕茧进行缫丝,即得到含纳米TiO2的桑蚕丝。
上述技术方案中,纳米二氧化钛的粒径为1~100 nm。
上述技术方案中,步骤(2)中的晾干为室温下自然晾干。
上述技术方案中,步骤(2)中添食家蚕时的给桑量和平常使用量一样。添食带有TiO2的适熟叶后的家蚕常规饲养、上蔟。步骤(3)中的缫丝属于现有技术。
本发明结合家蚕的生理特征,开发了蚕用纳米添加剂;步骤(1)中制备的添加剂溶液在使用前充分混匀,按照100kg桑叶添加1.0L剂量均匀喷洒适熟叶,量少会影响使用效果,量高会增加使用成本;待适熟叶自然晾干后添食家蚕,避免食下水份过多,影响饲料的消化和吸收,给桑量和平常使用量一样;纳米添加剂可以和其他蚕药及添加剂混合使用,不用影响使用效果。
桑蚕合成丝蛋白的主要时期是五龄第3天以后(第3天以前主要合成蚕体蛋白),在桑蚕丝蛋白大量合成的时候,使桑蚕体内存在大量的纳米TiO2,就能够在将纳米TiO2和用于合成丝蛋白的氨基酸一起转运到桑蚕丝腺,在丝蛋白的合成和分泌过程中含有一定量的纳米TiO2,并且这些纳米TiO2不是简单附着于丝蛋白表面,而是和丝蛋白得到了均匀混合,这对于改良桑蚕丝蛋白的性能。
本发明通过测定单位质量桑蚕丝(g)中Ti元素的含量(ng)进行评定桑蚕丝中的纳米TiO2的含量;Ti元素的含量采用电感耦合等离子体光谱(ICP-S)法测量。
由于上述技术方案运用,本发明具有下列优点:
1.本发明首次不采用化学方法,将纳米TiO2嵌入桑蚕丝蛋白,桑蚕丝中的纳米TiO2含量高,分布均匀,更加稳定;水洗50次后,桑蚕丝中的纳米TiO2几乎没有损失,留存率最高达95%。
2. 本发明从丝蛋白大量合成的五龄第3天起连续添食纳米TiO2,通过家蚕对纳米TiO2的吸收,使家蚕体内存在大量的纳米TiO2,在丝蛋白合成时,纳米TiO2直接嵌入丝蛋白,达到制备含有纳米TiO2桑蚕丝的目的。
3.本发明公开的方法中使用的添加剂用量少、来源广泛、成本低;无需改变生产规律,操作方便,易于推广应用,不会对环境产生影响。
具体实施方式
下面结合实施例对本发明作进一步描述:
实施例一:一种含纳米TiO2桑蚕丝的制备方法
⑴ 材料及药品:
桑蚕品种:苏秀×春丰,取得了江苏省蚕品种审定委员会颁发的蚕品种证书(苏审蚕201001),具有家蚕的基本共性。
药品:纳米TiO2为杭州万景新材料有限公司公司产品。
其他分子生物学试剂为生工生物工程(上海)股份有限公司产品。
⑵ 纳米TiO2的使用
取纳米TiO2与水混合配制成浓度为150.0 mg/L的添加剂溶液;使用前充分混匀添加剂,按照100 kg桑叶添加1.0L剂量进行喷洒各龄期的适熟叶,桑树品种为育711,待适熟叶晾干后,对发育至五龄第3天的桑蚕进行连续添食到上蔟,给桑量和平常使用量一样。
⑶ 缫丝
采用常规方法对桑蚕茧进行缫丝。
⑷ 丝质检测
分别取试验区(喂食纳米TiO2)和对照区(未喂食纳米TiO2)的桑蚕丝进行丝质检测,表1为丝质检测结果。
表1 丝质检测结果
项目 | 试验区 | 对照区 |
粒茧丝长(米) | 1732±21 | 1720±18 |
解舒率(%) | 75±3 | 74±3 |
纤度(D) | 2.231±0.27 | 2.241±0.27 |
净度(分) | 98.5 | 98.5 |
表1丝质检测结果表明,添食纳米TiO2后,丝质成绩和对照相当,各项指标都高于对照区。
⑸ 桑蚕丝中纳米TiO2含量及稳定性测定
桑蚕丝中纳米TiO2含量测定:分别取试验区(喂食纳米TiO2)和对照区(未喂食纳米TiO2)的桑蚕丝0.3g进行消化。首先,在桑蚕丝加入10mL浓硝酸(分析纯)过夜;然后,在反应液中加入0.5ml的H2O2,将反应液置于160℃的高压反应容器中加热,直至桑蚕丝完全溶解;在120℃继续加热溶液,消除剩余的硝酸,直到溶液为无色透明。随后在马弗炉中焙烧4小时,最后,用2%硝酸溶解,过滤后定容;将消化完毕的样品用电感耦合等离子体光谱(ICP-S)法测量组织中的钛含量,数据用ng(钛含量)/g(组织鲜重)表示(见表2)。
纳米TiO2稳定性测定:将制备的含有纳米TiO2桑蚕丝经水洗50次后,再采用上述的纳米TiO2含量测定方法进行测定(见表2)。
表2桑蚕丝中纳米TiO2含量测定结果
试验区 | 对照区 | |
桑蚕丝中Ti含量(ng/g) | 500±25 | 0 |
水洗50次桑蚕丝中Ti含量(ng/g) | 465±30 | - |
表2表明,对五龄第3天的桑蚕连续添食纳米TiO2后,生产的桑蚕丝中含量大量的纳米TiO2,经水洗50次后,留存率达93%,证明该发明为桑蚕丝的改性提供了一种可行的方法。
实施例二:一种含纳米TiO2桑蚕丝的制备方法
⑴ 材料及药品:
桑蚕品种:苏秀×春丰,取得了江苏省蚕品种审定委员会颁发的蚕品种证书(苏审蚕201001),具有家蚕的基本共性。
药品:纳米TiO2为杭州万景新材料有限公司公司产品。
其他分子生物学试剂为生工生物工程(上海)股份有限公司产品。
⑵ 纳米TiO2的使用
取纳米TiO2与水混合配制成浓度为100.0 mg/L的添加剂溶液;使用前充分混匀添加剂,按照100 kg桑叶添加1.0L剂量进行喷洒各龄期的适熟叶,桑树品种为育711,待适熟叶晾干后,对发育至五龄第3天的桑蚕进行连续添食到上蔟,给桑量和平常使用量一样。
⑶ 缫丝
采用常规方法对桑蚕茧进行缫丝。
⑷ 丝质检测
分别取试验区(喂食纳米TiO2)和对照区(未喂食纳米TiO2)的桑蚕丝进行丝质检测,表3为丝质检测结果。
表3 丝质检测结果
试验区 | 对照区 | |
粒茧丝长(米) | 1742±20 | 1728±16 |
解舒率(%) | 76±2 | 75±4 |
纤度(D) | 2.219±0.19 | 2.221±0.20 |
净度(分) | 98.5 | 98.5 |
表3丝质检测结果表明,添食纳米TiO2后,丝质成绩和对照相当,各项指标都略高于对照区。
⑸ 桑蚕丝纳米TiO2含量及稳定性测定
纳米TiO2含量测定:分别取试验区(喂食纳米TiO2)和对照区(未喂食纳米TiO2)桑蚕丝0.3g进行消化。首先,在桑蚕丝加入10mL浓硝酸(分析纯)过夜。然后,在反应液中加入0.5ml的H2O2,将反应液置于160℃的高压反应容器中加热,直至桑蚕丝块完全溶解。在120℃继续加热溶液,消除剩余的硝酸,直到溶液为无色透明。随后在马弗炉中焙烧4小时,最后,用2%硝酸溶解,过滤后定容。将消化完毕的样品用电感耦合等离子体光谱(ICP-S)法测量组织中的钛含量,数据用ng(钛含量)/g(组织鲜重)表示(见表4)。
纳米TiO2稳定性测定:将制备的含有纳米TiO2桑蚕丝经水洗50次后,再采用上述的纳米TiO2含量测定方法进行测定(见表4)。
表4桑蚕丝中纳米TiO2含量测定结果
试验区 | 对照区 | |
桑蚕丝中TiO2含量(ng/g) | 440±21 | 0 |
水洗50次桑蚕丝中TiO2含量(ng/g) | 418±19 | - |
表4表明,对五龄第3天的桑蚕连续添食浓度较低的纳米TiO2添加剂溶液后,生产的桑蚕丝中也含有纳米TiO2,较实施例一低60ng/g左右,经水洗50次后,留存率达95%,表明桑蚕丝中含量较低的纳米TiO2,经水洗后的留存率较高。
Claims (4)
1.一种含纳米TiO2桑蚕丝的制备方法,其特征在于,包括如下步骤:
(1) 添加剂溶液的配制:将纳米TiO2与水进行混合后配制成浓度为100~150mg/L的添加剂溶液;
(2) 添食家蚕:将步骤(1)中制备的添加剂溶液按照100kg桑叶添加1L溶液剂量喷洒适熟叶,待适熟叶晾干后,对发育到五龄第3天的家蚕连续添食至上蔟;
(3) 缫丝:对步骤(2)中生长至上蔟阶段的家蚕蚕茧进行缫丝,即得到含纳米TiO2的桑蚕丝。
2.根据权利要求1所述含纳米TiO2桑蚕丝的制备方法,其特征在于:纳米二氧化钛的粒径为1~100 nm。
3.根据权利要求1所述含纳米TiO2桑蚕丝的制备方法,其特征在于:步骤(2)中的晾干为室温下自然晾干。
4.根据权利要求1所述含纳米TiO2桑蚕丝的制备方法,其特征在于:步骤(2)中添食家蚕时的给桑量和平常使用量一样。