CN103923533A - Wall paint for children and preparation method thereof - Google Patents

Wall paint for children and preparation method thereof Download PDF

Info

Publication number
CN103923533A
CN103923533A CN201410144596.2A CN201410144596A CN103923533A CN 103923533 A CN103923533 A CN 103923533A CN 201410144596 A CN201410144596 A CN 201410144596A CN 103923533 A CN103923533 A CN 103923533A
Authority
CN
China
Prior art keywords
children
wall paint
parts
add
thickening material
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201410144596.2A
Other languages
Chinese (zh)
Inventor
钟志杰
戴文英
张进风
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
HESHAN MICKEY PAINT Co Ltd
Original Assignee
HESHAN MICKEY PAINT Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by HESHAN MICKEY PAINT Co Ltd filed Critical HESHAN MICKEY PAINT Co Ltd
Priority to CN201410144596.2A priority Critical patent/CN103923533A/en
Publication of CN103923533A publication Critical patent/CN103923533A/en
Pending legal-status Critical Current

Abstract

The invention discloses wall paint for children and a preparation method thereof. The wall paint for children consists of the following components in parts by weight: 10-30 parts of tap water, 0.1-0.5 part of wetting agent, 0.3-1.5 parts of dispersing agent, 0.3-1 part of defoaming agent, 1-6 parts of photocatalyst, 1-3 parts of thickener, 10-30 parts of titanium dioxide powder, 15-40 parts of filler and 30-50 parts of VAE (Vinyl Acetate Ethylene) Emulsion. The invention further discloses a preparation method of the wall paint for children. The wall paint for children contains low-VOC (Volatile Organic Compound) odor-free paint liquid. After a paint film is formed, the air can be purified effectively through a photo-catalytic reaction, the air quality is improved, and a healthy residential environment is provided of children. The wall paint for children is reliable in quality.

Description

A kind of children's wall paint and preparation method thereof
Technical field
The present invention relates to paint field, refer to especially a kind of children's wall paint.
Background technology
Wall paint is requisite Chemicals during people live.In recent years, people's environmental consciousness strengthens day by day, various environment protection type wall covering paints arise at the historic moment, as Chinese invention patent CN200610127348.2 provides a kind of environmental protection wall surface paint, by selecting the emulsion of low VOC, reduce the content of objectionable impurities, simultaneously by adding harmless additive, the content that has reduced VOC in product and formaldehyde, is of value to and builds healthy comfortable living environment.Chinese invention patent CN201210525972.3 discloses a kind of super purification wall paint and preparation method thereof, and this invention adopts the clean taste emulsion of VAE, and has added natural diatomaceous earth, ultra-fine filling material, has the effect of low VOC discharge, waterproof, protection against the tide.
Children are special consumer groups, and living environment direct relation growing up healthy and sound of each child, and the quality of wall paint plays an important role to living environment.Although above-described environmental protection wall surface paint has reduced the content of objectionable impurities in wall paint, cannot purify air, and cannot solve the problems such as living environment atmospheric pollution, finishing pollution.Therefore, there is the novel environment friendly children wall paint that improves Air quality, air purification function and become new research direction.
Summary of the invention
The present invention proposes a kind of children's wall paint and preparation method thereof, has purifying air, improves the effect of Air quality.
Technical scheme of the present invention is achieved in that
A kind of children's wall paint, each moiety and parts by weight are: tap water 10-30 part, environment-friendly type wetting agent 0.1-0.5 part, dispersion agent 0.3-1.5 part, defoamer 0.3-1 part, photocatalyst 1-6 part, thickening material 1-3 part, titanium dioxide 10-30 part, filler 15-40 part, vinyl acetate/ethylene copolymerization emulsions (hereinafter to be referred as VAE emulsion) 30-50 part.
Further, described wetting agent is moistening dose of environment-friendly type.
Further, described dispersion agent is sodium salt dispersion agent.
Further, described thickening material is cellulose thickener and polyurethanes thickening material.
Further, described thickening material composition and parts by weight are: cellulose thickener 0.5-2 part, polyurethanes thickening material 0.5-1 part.
The present invention also provides a kind of method of preparing this children's wall paint, comprises the following steps:
(1) tap water, environment-friendly type wetting agent, sodium salt dispersion agent, defoamer, photocatalyst are weighed and are added in Scattered Kettle by formula.
(2) titanium dioxide, filler are weighed and are added in Scattered Kettle.
(3) add the cellulose thickener of weighing by formula.
(4) in dispersion mill, carrying out high speed dispersion is ground to fineness and is less than 50 μ m.
(5) polyurethanes thickening material and VAE emulsion are weighed by formula, and slowly add low speed in Scattered Kettle to disperse 5 ~ 10 minutes.
(6) inspection, filtration, packaging.
The invention has the beneficial effects as follows:
A kind of children's wall paint that the present invention proposes, there is the clean taste paint of low VOC liquid, after its paint film moulding, photocatalyst in component is under the effect of light, the poisonous and hazardous gas in air of effectively degrading also has the function of sterilization, deodorizing, mildew-resistant simultaneously, can effectively purify air, improve Air quality, for children provide a healthy living environment.For the children disease causing because of atmospheric pollution, especially respiratory system disease, has the effect of assisting therapy.
The present invention also provides the preparation method of described children's wall paint, applies children's wall paint prepared by the method, has improved the consistency of storeroom, does not produce the phenomenons such as flocculation, reunion, reliable product quality.
Embodiment
Below in conjunction with the embodiment of the present invention, the technical scheme in the present invention is clearly and completely described, obviously, described embodiment is only the present invention's part embodiment, instead of whole embodiment.Based on the embodiment in the present invention, those of ordinary skill in the art, not making the every other embodiment obtaining under creative work prerequisite, belong to the scope of protection of the invention.
Below in conjunction with embodiment, further set forth the present invention:
Embodiment 1
(1) take tap water 100 kg, environment-friendly type wetting agent 1 kg, sodium salt dispersion agent 3 kg, defoamer 3 kg, photocatalyst 10 kg weigh and add in Scattered Kettle by formula.
(2) take titanium dioxide 100 kg, filler 150 kg add in Scattered Kettle.
(3) add cellulose thickener 5 kg.
(4) in dispersion mill, carrying out high speed dispersion is ground to fineness and is less than 50 μ m.
(5) take polyurethanes thickening material 5 kg, VAE emulsion 300 kg, slowly add low speed in Scattered Kettle to disperse 5 ~ 10 minutes.
(6) inspection, filtration, packaging.
Embodiment 2
(1) take tap water 200 kg, environment-friendly type wetting agent 3 kg, sodium salt dispersion agent 9 kg, defoamer 6 kg, photocatalyst 30 kg, add in Scattered Kettle.
(2) take titanium dioxide 220 kg, filler 240 kg, add in Scattered Kettle.
(3) add cellulose thickener 13 kg.
(4) in dispersion mill, carrying out high speed dispersion is ground to fineness and is less than 50 μ m.
(5) take polyurethanes thickening material 7 kg, VAE emulsion 400 kg, slowly add low speed in Scattered Kettle to disperse 5 ~ 10 minutes.
(6) inspection, filtration, packaging.
Embodiment 3
(1) take tap water 300 kg, environment-friendly type wetting agent 5 kg, sodium salt dispersion agent 15 kg, defoamer 10 kg, photocatalyst 60 kg, add in Scattered Kettle.
(2) take titanium dioxide 300 kg, filler 400 kg, add in Scattered Kettle.
(3) add cellulose thickener 20 kg.
(4) in dispersion mill, carrying out high speed dispersion is ground to fineness and is less than 50 μ m.
(5) take polyurethanes thickening material 10 kg, VAE emulsion 500 kg, slowly add low speed in Scattered Kettle to disperse 5 ~ 10 minutes.
(6) inspection, filtration, packaging.
Embodiment 4
(1) take tap water 200 kg, environment-friendly type wetting agent 3 kg, sodium salt dispersion agent 9 kg, defoamer 6 kg, photocatalyst 30 kg, add in Scattered Kettle.
(2) take titanium dioxide 220 kg, filler 240 kg, add in Scattered Kettle.
(3) add cellulose thickener 10 kg.
(4) in dispersion mill, carrying out high speed dispersion is ground to fineness and is less than 50 μ m.
(5) take polyurethanes thickening material 10 kg, VAE emulsion 500 kg, slowly add low speed in Scattered Kettle to disperse 5 ~ 10 minutes.
(6) inspection, filtration, packaging.
Embodiment 5
(1) take tap water 200 kg, environment-friendly type wetting agent 3 kg, sodium salt dispersion agent 9 kg, defoamer 6 kg, photocatalyst 30 kg, add in Scattered Kettle.
(2) take titanium dioxide 220 kg, filler 240 kg, add in Scattered Kettle.
(3) add cellulose thickener 15 kg.
(4) in dispersion mill, carrying out high speed dispersion is ground to fineness and is less than 50 μ m.
(5) take polyurethanes thickening material 10 kg, VAE emulsion 400 kg, slowly add low speed in Scattered Kettle to disperse 5 ~ 10 minutes.
(6) inspection, filtration, packaging.
Embodiment 6
(1) take tap water 300 kg, environment-friendly type wetting agent 5 kg, sodium salt dispersion agent 15 kg, defoamer 10 kg, photocatalyst 60 kg, add in Scattered Kettle.
(2) take titanium dioxide 30 kg, filler 400 kg, add in Scattered Kettle.
(3) add cellulose thickener 15 kg.
(4) in dispersion mill, carrying out high speed dispersion is ground to fineness and is less than 50 μ m.
(5) take polyurethanes thickening material 10 kg, VAE emulsion 500 kg, slowly add low speed in Scattered Kettle to disperse 5 ~ 10 minutes.
(6) inspection, filtration, packaging.
Embodiment 7
(1) take tap water 300 kg, environment-friendly type wetting agent 5 kg, sodium salt dispersion agent 15 kg, defoamer 10 kg, photocatalyst 60 kg, add in Scattered Kettle.
(2) take titanium dioxide 30 kg, filler 400 kg, add in Scattered Kettle.
(3) add cellulose thickener 20 kg.
(4) in dispersion mill, carrying out high speed dispersion is ground to fineness and is less than 50 μ m.
(5) take polyurethanes thickening material 5 kg, VAE emulsion 500 kg, slowly add low speed in Scattered Kettle to disperse 5 ~ 10 minutes.
(6) inspection, filtration, packaging.
Wherein, wetting agent can reduce surface tension or interfacial tension, and make water can more easily be deployed in solid materials surface and penetrate its surface and soaked, be the requisite auxiliary agent of coating.Wetting agent contains a large amount of solvents more, becomes one of source of VOC.The wetting agents of EW-10, HT100, EW-107 novel environment-friendly etc. are due to containing APEO and VOC, and have good surfactivity and wettability, are more and more applied to every field.Children's wall paint that the present invention proposes is selected the wetting agent of the acceptable environment-friendly type of coating industry, reduces the discharge of VOC.
Adding of dispersion agent can reduce jitter time, improves gloss, improves tinting strength and opacifying power, improves color developing and toning property, prevents flocculation and sedimentation.What the dispersion agent major part that coating is used was used belongs to negatively charged ion and non-ionic dispersing agent.In actual production, it is many that sodium salt dispersion agent and ammonium salt dispersion agent use.Ammonium salt dispersion agent water-tolerant, bad dispersibility; And sodium salt dispersion agent good dispersity, poor water resistance.Children's wall paint of the present invention, the characteristic of comprehensive evaluation dispersion agent, selects sodium salt dispersion agent.
The wetting agent that the present invention selects and dispersion agent all belong to tensio-active agent, easily bubble aborning, therefore need to add defoamer.Defoamer is of a great variety, can be divided into by composition: natural fats and oils, polyethers defoamer, higher alcohols, silicon class, polyether-modified silicon, novel self-emulsifying defoamer, polysiloxane defoamers etc.Children's wall paint of the present invention is selected acceptable defoamer in coating, and kind is not done requirement.
Titanium dioxide main component is titanium dioxide (T io 2), be a kind of polycrystalline compounds, its particle becomes regularly arranged, has grid system.Titanium dioxide stable chemical nature, conventional in industry have anatase titanium dioxide (A type) and rutile-type (R) type.Titanium dioxide is considered at present the best a kind of white pigment of performance in the world, is widely used in the industries such as coating, plastics, papermaking, chemical fibre, makeup.Compared with other white pigments, titanium dioxide has superior whiteness, tinting strength, opacifying power, weathering resistance, thermotolerance and chemical stability.Children's wall paint of the present invention has added titanium dioxide, and product color is bright-coloured, and can amplified medium stability and paint film physical strength and sticking power, prevents crackle, prevents that ultraviolet ray and moisture from seeing through, and can extend coating work-ing life.
Thickening material mainly contains cellulose family, polyacrylate dispersion class and association type polyurethanes thickening material 3 classes.Cellulose family is few to formulation for coating material restriction, but stability is bad, and not only to paint flow, sex change exerts an influence polyurethanes, and and adjacent latex particle between exist and interact.Therefore children's wall paint thickening material cellulose family of the present invention and polyurethanes allotment are used, in production process, first add cellulose thickener, then add polyurethanes thickening material, give full play to the advantage of two kinds of thickening materials, strengthen product stability, improve product quality.
Photocatalyst is a kind of general name of the semiconductor material with photo-catalysis function, taking Nano titanium dioxide as representative.Photocatalyst is coated substrate surface, under the effect of light, can produce free hydroxy and active oxygen, dissociates to removing airborne flue dust in air, go mouldy, and improves Air quality.The photocatalyst airborne toxic and harmful of can also effectively degrading, as formaldehyde, benzene etc., effectively administers finishing pollution problem; Intestinal bacteria, streptococcus aureus, avian influenza virus etc. are all had to certain restraining effect, and the toxin of energy bacterium for degrading generation, purify air, improve habitation environment quality.Children's wall paint provided by the invention adopts clean taste paint liquid simultaneously, adds photocatalyst technology, greatly reduce product VOC content, there is the functions such as degraded toxic and harmful, antibacterial, deodorizing, mildew-resistant simultaneously, improve living environment Air quality, met the children's that Air quality is had relatively high expectations demand.
The foregoing is only preferred embodiment of the present invention, in order to limit the present invention, within the spirit and principles in the present invention not all, any amendment of doing, be equal to replacement, improvement etc., within all should being included in protection scope of the present invention.

Claims (5)

1. children's wall paint, it is characterized in that, each moiety and parts by weight are: tap water 10-30 part, wetting agent 0.1-0.5 part, dispersion agent 0.3-1.5 part, defoamer 0.3-1 part, photocatalyst 1-6 part, thickening material 1-3 part, titanium dioxide 10-30 part, filler 15-40 part, vinyl acetate/ethylene copolymerization emulsions (hereinafter to be referred as VAE emulsion) 30-50 part.
2. a kind of children's wall paint according to claim 1, is characterized in that: described wetting agent is moistening dose of environment-friendly type.
3. a kind of children's wall paint according to claim 1, is characterized in that: described dispersion agent is sodium salt dispersion agent.
4. a kind of children's wall paint according to claim 1, is characterized in that: described thickening material composition and parts by weight are: cellulose thickener 0.5-2 part, polyurethanes thickening material 0.5-1 part.
5. the method for preparation a kind of children's wall paint claimed in claim 1, is characterized in that the method comprises the following steps:
(1) add in Scattered Kettle by weigh tap water, environment-friendly type wetting agent, sodium salt dispersion agent, defoamer, photocatalyst of formula;
(2) weigh and add in Scattered Kettle by weigh titanium dioxide, filler of formula;
(3) add the cellulose thickener of weighing by formula;
(4) in dispersion mill, carrying out high speed dispersion is ground to fineness and is less than 50 μ m;
(5) polyurethanes thickening material and VAE emulsion are weighed by formula, and slowly add low speed in Scattered Kettle to disperse 5 ~ 10 minutes;
(6) inspection, filtration, packaging.
CN201410144596.2A 2014-04-11 2014-04-11 Wall paint for children and preparation method thereof Pending CN103923533A (en)