CN103831172A - Combination collecting agent and method for improving antimony, lead and associated silver flotation recovery rate by adopting combination collecting agent - Google Patents

Combination collecting agent and method for improving antimony, lead and associated silver flotation recovery rate by adopting combination collecting agent Download PDF

Info

Publication number
CN103831172A
CN103831172A CN201410121821.0A CN201410121821A CN103831172A CN 103831172 A CN103831172 A CN 103831172A CN 201410121821 A CN201410121821 A CN 201410121821A CN 103831172 A CN103831172 A CN 103831172A
Authority
CN
China
Prior art keywords
antimony
collecting agent
lead
zinc
black powder
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201410121821.0A
Other languages
Chinese (zh)
Other versions
CN103831172B (en
Inventor
刘建军
丁大森
欧阳金德
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Lhasa Weizhuo Rock And Mineral Analysis & Testing Co Ltd
TIBET HUAYU MINING Co Ltd
Original Assignee
Lhasa Weizhuo Rock And Mineral Analysis & Testing Co Ltd
TIBET HUAYU MINING Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Lhasa Weizhuo Rock And Mineral Analysis & Testing Co Ltd, TIBET HUAYU MINING Co Ltd filed Critical Lhasa Weizhuo Rock And Mineral Analysis & Testing Co Ltd
Priority to CN201410121821.0A priority Critical patent/CN103831172B/en
Publication of CN103831172A publication Critical patent/CN103831172A/en
Application granted granted Critical
Publication of CN103831172B publication Critical patent/CN103831172B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention relates to a combination collecting agent. The combination collecting agent is composed of amyl sodium xanthate, 25 # black powder and butyl ammonium black powder; the weight ratio of the amyl sodium xanthate, the 25 # black powder and the butyl ammonium black powder is 2-5:20-35:15-30. By the adoption of the combination collecting agent, the antimony lead and associated silver flotation recovery rate can be greatly increased during flotation, the antimony and lead recovery rate is kept above 49% and can reach 59.09%, the lead recovery rate can reach 94.44%, the antimony recovery rate can reach 65.78%, the silver recovery rate can reach 88.31%, and the effect is obvious. In addition, the combination collecting agent can be adopted for operation under the situation that an original production technology is not changed, agentia is easy to add, the use rate of mineral resources is greatly increased, and the non-poisonous and non-pollution effect is achieved.

Description

A kind of combined capturing and collecting agent and employing combined capturing and collecting agent thereof improve the method for antimony lead and associated silver flotation recovery rate
Technical field
The present invention relates to flotation from plumbous many metals of zinc antimony raw ore and reclaim antimony lead and associated silver; The present invention be more particularly directed to a kind of combined capturing and collecting agent and adopt combined capturing and collecting agent to improve the method for antimony lead and associated silver flotation recovery rate.
Background technology
Sangri mining area is positioned at Tibet Autonomous Region Longzi County, is the plumbous zinc multi-metal complex sulphide ore of the ultra-large type base that Tibet Autonomous Region finds up to now; In this region, plumbous many metals of zinc raw ore embedding cloth is related to complexity, and granule size thickness inequality belongs to complex refractory ore.In ore, main antimony mineral is boulangerite, jamesonite, and galena, stibnite are few; Zinc mineral is mainly zincblende; Silver mineral is mainly silver-colored antimony tetrahedrite.Jamesonite, boulangerite have corrosion explanation phenomenon in various degree to galena, zincblende, pyrite, monomer dissociation difficulty, therefore current output lead antimony compound refined mine and zinc concentrate.
Along with mineral resources are exploited in a large number, the main feature of poor, thin, the assorted tcrude ore resource that is current exploitation.In this raw ore, jamesonite is compared with galena, have the advantages that disseminated grain size is thin, floatability is poor, and silver mineral is except main silver-colored antimony tetrahedrite, the main carriers mineral of other associated silver are boulangerite, jamesonite and galena etc., and therefore effectively improving antimony, the plumbum floatation rate of recovery is the Important Action that associated silver is reclaimed in strengthening.Lot of experiments is studied with practice and is shown, in this raw ore, boulangerite, jamesonite are to flotation pH value sensitivity, and experimental study is consistent with production practices to be shown, this raw ore of flotation is more suitable under the condition of neutral pH=7.0 ~ 7.5, and plumbous antimony flotation recovery rate is higher ;owing to containing a certain amount of zinc mineral in raw ore, therefore can not infinitely strengthen collector dosage strengthening collecting effect in preferential floating plumbous antimony operation, say again, if excessive collecting agent pours in the selected operation of plumbous antimony, its lead-antimony concentrate grade is by uncontrollable, and lead adds antimony grade and cannot remain on more than 45%, so not only affects Business Economic Benefit, also increase Product transport cost, directly had influence on the economic benefit of downstream smelting enterprise simultaneously.
For example application number is 201010614789.1, publication number is the Chinese invention patent " a kind of method that improves argillization high-sulfur jamesonite Floatation Concentrate Grade " of CN102218375A, this patent discloses a kind of method that improves argillization high-sulfur jamesonite Floatation Concentrate Grade, the method need to, by adding the specific inhibitors such as tannin extract, improve lead-antimony concentrate grade; Cause floatation process step complexity, and cost of investment is high; And the lead floatingly selecting adds that antimony grade is the highest can only arrive 48.03%, lead adds that antimony recovery is the highest can only arrive 77.34%.
For example application number is 201310413919.9 again, publication number is the Chinese invention patent " method for floating of the complicated jamesonite of a kind of microfine " of CN103433142A, this patent discloses the method for floating of the complicated jamesonite of a kind of microfine, comprise that carbon plumbously separates, plumbous mud separates, plumbous sulphur content from; The method need to adopt special separating technology to obtain product; Special separating technology causes flotation cost of investment high, and the lead floatingly selecting adds that antimony grade is the highest can only arrive 43.5%, and lead adds that antimony recovery is the highest can only arrive 66.12%.
Summary of the invention
The object of the invention is to overcome the problems referred to above that prior art exists, propose a kind of combined capturing and collecting agent and adopt combined capturing and collecting agent to improve the method for antimony lead and associated silver flotation recovery rate.It is under 7 ~ 7.5 condition that the present invention can be applicable to slurry pH, using zinc sulfate and sodium sulfite as zinc sulphide and pyritous inhibitor, then adds combined capturing and collecting agent; In flotation, can make the flotation recovery rate of antimony lead and associated silver increase substantially, lead adds antimony grade and remains on more than 49%, and lead adds antimony grade can reach 59.09%, and lead recovery can reach 94.44%, antimony recovery can reach 65.78%, silver raising recovery rate 88.31%, and effect is remarkable; The present invention adopts combined capturing and collecting agent in the situation that not changing original production technology, to operate, and medicament adds easy to implement, has greatly improved Utilization Rate of Mineral Resources, and nontoxic pollution-free.
The present invention realizes by the following technical solutions:
A kind of combined capturing and collecting agent, is characterized in that: comprise amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 2 ~ 5:20 ~ 35:15 ~ 30.
When use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with to weight percent concentration and are 1 ~ 5% the aqueous solution, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add to respectively in ore pulp simultaneously.
Adopt combined capturing and collecting agent to improve a method for antimony lead and associated silver flotation recovery rate, it is characterized in that the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous many metals of zinc antimony raw ore through broken, be ground to after mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate and the sodium sulfite that suppress zinc, sulfur mineral in ore pulp, after fully stirring; Add galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral are combined to the combined capturing and collecting agent of collecting, combination collecting obtains lead-antimony concentrate product.In floatation process by 25 #black powder, amyl group sodium xanthate and aerofloat 226 add respectively mixing in ore pulp simultaneously to and use, and can give full play to the cooperative effect between medicament.
Zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; In combined capturing and collecting agent 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
By 1 ton of plumbous many metals of zinc antimony raw ore, when flotation: zinc sulfate consumption is 400 ~ 1100g, sodium sulfite
Consumption is 90 ~ 180g, and combined capturing and collecting agent consumption is 370 ~ 700g.
When use, respectively zinc sulfate and sodium sulfite are mixed with to weight percent concentration and are 5 ~ 10% the aqueous solution, more respectively amyl group sodium xanthate and aerofloat 226 to be mixed with to weight percent concentration be 1 ~ 5% the aqueous solution, and 25 #black powder is stoste; First in ore pulp, add the zinc sulfate solution and the sodium sulfite aqueous solution that suppress zinc, sulfur mineral, after fully stirring; In ore pulp, add respectively the amyl group sodium acrinol solution, 25 that galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral is combined to collecting more simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
Add and refer at one time respectively simultaneously, separately amyl group sodium acrinol solution is joined in ore pulp, separately by 25 #black powder stoste joins in ore pulp and separately the aerofloat 226 aqueous solution is joined in ore pulp.
Amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 23:306:157.
Amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 28:266:197.
Amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 35:237:219.
Described fragmentation refers to the fine ore that plumbous many metals of zinc antimony crushing raw ore is less than to 12 millimeters to granularity; Described grinding refers to that adopting ore mill that granularity is less than to the fine ore of 12 millimeters is ground to after mineral disaggregation, forms the ore pulp that pH value is 7 ~ 7.5.
25 #black powder is the conventional collecting agent of the sulphide ores such as lead, copper, silver.
Compared with prior art, its advantage is in the present invention:
1, to can be applicable to slurry pH be under 7 ~ 7.5 condition in the present invention, using zinc sulfate and sodium sulfite as zinc sulphide and pyritous inhibitor, then adds combined capturing and collecting agent; In flotation, can make the flotation recovery rate of antimony lead and associated silver increase substantially, lead adds antimony grade and remains on more than 49%, and lead adds antimony grade can reach 59.09%, and lead recovery can reach 94.44%, antimony recovery can reach 65.78%, silver raising recovery rate 88.31%, and effect is remarkable; The present invention adopts combined capturing and collecting agent in the situation that not changing original production technology, to operate, and medicament adds easy to implement, has greatly improved Utilization Rate of Mineral Resources, and nontoxic pollution-free.
2, the present invention in use, 25 #black powder is that stoste is added; Respectively amyl group sodium xanthate and aerofloat 226 are mixed with to the aqueous solution, the aqueous solution of amyl group sodium xanthate 1 ~ 5% weight percent concentration; The aqueous solution of aerofloat 226 1 ~ 5% weight percent concentration; First amyl group sodium xanthate and aerofloat 226 are mixed with to the aqueous solution, amyl group sodium acrinol solution and 25 #black powder can be accelerated the reaction of galena in ore pulp, jamesonite and stibnite, strengthening collecting effect; Aerofloat 226 can be accelerated the reaction of silver-colored antimony tetrahedrite and association silver ore in ore pulp, improves the ascent rate of silver-colored antimony tetrahedrite and association silver ore in ore pulp, thereby improves collecting effect and the combination collecting rate of combined capturing and collecting agent.
3, medicament of the present invention is conventional dose, and medicament use amount is few, and cost is low, and nontoxic pollution-free; The on-the-spot application of the present invention is easy to implement; Can in the situation that not changing original production technology, operate, avoid the technological process of change produced on-site, cause that cost of investment is high, field conduct complicated situation occurs.
4, the present invention adopts 25 #black powder, amyl group sodium xanthate and aerofloat 226 combine rear interpolation in specific proportions, and concrete principle is: 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and association silver ore, carried out the commerical test of 1 year 2500t/d by above-mentioned technological parameter, result shows to adopt combinations thereof collecting agent dosage regimen can effectively carry the flotation recovery rate of high lead-antimony and associated silver, obtain lead-antimony concentrate: lead adds antimony grade and can reach and can reach 59.09%, lead recovery can reach 94.44%, antimony recovery can reach 65.78%, silver raising recovery rate 88.31%, and effect is remarkable.
5, the present invention compared with prior art, do not need to add the adjusting agents such as large quantities of lime and remove deliberately to change pulp PH value, and the consumption of zinc sulfate and sodium sulfite is few, the lead that adopts method of the present invention to floatingly select adds antimony grade can reach 59.09%, and lead recovery can reach 94.44%, antimony recovery can reach 65.78%, silver raising recovery rate 88.31%.
6, the present invention compares with " method for floating of the complicated jamesonite of a kind of microfine " with " a kind of method that improves argillization high-sulfur jamesonite Floatation Concentrate Grade " in background technology, the present invention adopts conventional beneficiation reagent completely, and head adds zinc sulfate and sodium sulfite inhibitor zinc, sulfur mineral; Add and comprise 25 again #the combined capturing and collecting agent of black powder, amyl group sodium xanthate and aerofloat 226 selectively mixes collecting to object mineral; 25 #the part by weight of black powder, amyl group sodium xanthate and aerofloat 226 is: 2 ~ 5:20 ~ 35:15 ~ 30, make full use of 25 #cooperative effect between black powder, amyl group sodium xanthate and the interaction of aerofloat 226, reaches the object of the flotation recovery rate that improves antimony lead and associated silver; With adopt compared with existing " a kind of method that improves argillization high-sulfur jamesonite Floatation Concentrate Grade " lead to add antimony grade to have improved 11.06%; Lead adds antimony grade and has improved 15.59% compared with adopting existing " method for floating of the complicated jamesonite of a kind of microfine "; Effect of the present invention is remarkable.
7, the present invention adopts amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 23:306:157; Carry out the commerical test of 1 year 300t/d by technique of the present invention and combined capturing and collecting agent administration conditional parameter, result shows effectively to carry the flotation recovery rate of high lead-antimony and associated silver, the plumbous antimony flow process of diffeential floatation of adopt one roughing, scan for three times, four times are selected, flotation of lead antimony mine tailing flotation zinc again.In the lead-antimony concentrate of obtaining in leaded 3.15%, antimony 1.48%, zinc 3.75%, sulphur 5.73%, silver-colored 255.77g/t, carbon content reach 1.49% ore pulp: lead adds antimony grade 49.05%, argentiferous 3089.4g/t, lead recovery 78.42%, antimony recovery 64.82%, silver raising recovery rate 84.45%.
8, the present invention adopts amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 28:266:197; Carry out the commerical test of 1 year 2000t/d by technique of the present invention and combined capturing and collecting agent administration conditional parameter, result shows effectively to carry the flotation recovery rate of high lead-antimony and associated silver, the plumbous antimony flow process of diffeential floatation of adopt one roughing, scan for three times, four times are selected, flotation of lead antimony mine tailing flotation zinc again.In the lead-antimony concentrate of obtaining in leaded 3.33%, antimony 1.05%, zinc 3.34%, sulphur 5.37%, silver-colored 163.45g/t, carbon content reach 1.52% ore pulp: lead adds antimony grade 59.09%, argentiferous 2257.16g/t, lead recovery 92.92%, antimony recovery 65.16%, silver raising recovery rate 88.31%.
9, the present invention adopts amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 35:237:219; Carry out the commerical test of 1 year 2500t/d by technique of the present invention and combined capturing and collecting agent administration conditional parameter, result shows effectively to carry the flotation recovery rate of high lead-antimony and associated silver, the plumbous antimony flow process of diffeential floatation of adopt one roughing, scan for three times, four times are selected, flotation of lead antimony mine tailing flotation zinc again.In the lead-antimony concentrate of obtaining in leaded 3.15%, antimony 0.94%, zinc 3.21%, sulphur 5.57%, silver-colored 144.17g/t, carbon content reach 1.61% ore pulp: lead adds antimony grade 56.89%, argentiferous 2010.75g/t, lead recovery 94.44%, antimony recovery 65.78%, silver raising recovery rate 88.09%.
10, the present invention adopts 25 #black powder and amyl group sodium xanthate, as the collecting agent of galena, jamesonite and stibnite, make antimony lead lock out operation steady, and aerofloat 226, as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral, makes silver-colored lock out operation steady; And 25 #cooperative effect between black powder, amyl group sodium xanthate and the interaction of aerofloat 226, can also improve the flotation recovery rate of antimony lead and associated silver.
Detailed description of the invention
By concrete enforcement example, technical scheme of the present invention is further described below.
Embodiment 1:
A kind of combined capturing and collecting agent, comprises amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 23:306:157.
When use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with to weight percent concentration and are 2.5% the aqueous solution, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add to respectively in ore pulp simultaneously.
The present invention is applied in a kind of method that adopts combined capturing and collecting agent raising antimony lead and associated silver flotation recovery rate, and the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous many metals of zinc antimony raw ore through broken, be ground to after mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate and the sodium sulfite that suppress zinc, sulfur mineral in ore pulp, after fully stirring; Add galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral are combined to the combined capturing and collecting agent of collecting, combination collecting obtains lead-antimony concentrate product.
Described fragmentation refers to the fine ore that plumbous many metals of zinc antimony crushing raw ore is less than to 12 millimeters to granularity; Described grinding refers to that adopting ore mill that granularity is less than to the fine ore of 12 millimeters is ground to after mineral disaggregation, forms the ore pulp that pH value is 7 ~ 7.5.
Zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; In combined capturing and collecting agent 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
The present invention is in the time of concrete application:
1, the former mineral material of the many metals of plumbous zinc antimony:
In the ore pulp forming: leaded 3.15%, antimony 1.48%, zinc 3.75%, sulphur 5.73%, silver-colored 255.77g/t, carbon content reach 1.49%; Pulp density 39.54%, a fineness-74 micron grade accounts for 80.85%; Plumbous antimony mainly exists with boulangerite and jamesonite form, and zinc is taking zincblende as main, and sulphur is taking pyrite and mispickel as main, and phosphorus content is higher, and fine particle stage material is than great.
2, floating agent and operating procedure:
Regime of agent:
By 1 ton of plumbous many metals of zinc antimony raw ore, in flotation: zinc sulfate consumption is 1057g, sodium sulfite consumption is 155g, and amyl group sodium xanthate consumption is 23g, 25 #black powder consumption is 306g, and aerofloat 226 consumption is 157g.
When use, first medicament is mixed with to following weight percent concentration:
Zinc sulfate 5% aqueous solution
Sodium sulfite 5% aqueous solution
Amyl group sodium xanthate 2.5% aqueous solution
25 #black powder stoste is added
Aerofloat 226 2.5% aqueous solution;
Operating procedure:
Plumbous many metals of zinc antimony raw ore micron grade to fineness-74 of regrinding after fragmentation is accounted for to 80.85%, the ore pulp that weight concentration is 39.54%; First in ore pulp, add inhibition zincblende and pyritous zinc sulfate solution and sodium sulfite aqueous solution, after fully stirring; In ore pulp, add respectively the amyl group sodium acrinol solution, 25 that galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral is combined to collecting more simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
Carried out the commerical test of 1 year 300t/d by above-mentioned technological parameter, result shows to adopt above-mentioned technique and combined capturing and collecting agent administration condition can effectively carry the flotation recovery rate of high lead-antimony and associated silver, the plumbous antimony flow process of diffeential floatation of adopt one roughing, scan for three times, four times are selected, flotation of lead antimony mine tailing flotation zinc again.In the lead-antimony concentrate of obtaining in leaded 3.15%, antimony 1.48%, zinc 3.75%, sulphur 5.73%, silver-colored 255.77g/t, carbon content reach 1.49% ore pulp: lead adds antimony grade 49.05%, argentiferous 3089.4g/t, lead recovery 78.42%, antimony recovery 64.82%, silver raising recovery rate 84.45%.
Embodiment 2:
A kind of combined capturing and collecting agent, comprises amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 28:266:197.
When use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with to weight percent concentration and are 2.5% the aqueous solution, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add to respectively in ore pulp simultaneously.
The present invention is applied in a kind of method that adopts combined capturing and collecting agent raising antimony lead and associated silver flotation recovery rate, and the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous many metals of zinc antimony raw ore through broken, be ground to after mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate and the sodium sulfite that suppress zinc, sulfur mineral in ore pulp, after fully stirring; Add galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral are combined to the combined capturing and collecting agent of collecting, combination collecting obtains lead-antimony concentrate product.
Described fragmentation refers to the fine ore that plumbous many metals of zinc antimony crushing raw ore is less than to 12 millimeters to granularity; Described grinding refers to that adopting ore mill that granularity is less than to the fine ore of 12 millimeters is ground to after mineral disaggregation, forms the ore pulp that pH value is 7 ~ 7.5.
Zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; In combined capturing and collecting agent 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
The present invention is in the time of concrete application:
1, the former mineral material of the many metals of plumbous zinc antimony:
In the ore pulp forming: leaded 3.33%, antimony 1.05%, zinc 3.34%, sulphur 5.37%, silver-colored 163.45g/t, carbon content reach 1.52%; Pulp density 38.79%, a fineness-74 micron grade accounts for 81.44%; Plumbous antimony mainly exists with boulangerite and jamesonite form, and zinc is taking zincblende as main, and sulphur is taking pyrite and mispickel as main, and phosphorus content is higher, and fine particle stage material is than great.
2, floating agent and operating procedure:
Regime of agent:
By 1 ton of plumbous many metals of zinc antimony raw ore, in flotation: zinc sulfate consumption is 864g, sodium sulfite consumption is 178g, and amyl group sodium xanthate consumption is 28g, 25 #black powder consumption is 266g, and aerofloat 226 consumption is 197g.
When use, first medicament is mixed with to following weight percent concentration:
Zinc sulfate 5% aqueous solution
Sodium sulfite 5% aqueous solution
Amyl group sodium xanthate 2.5% aqueous solution
25 #black powder stoste is added
Aerofloat 226 2.5% aqueous solution;
Operating procedure:
Micron grade to fineness-74 of first plumbous many metals of zinc antimony raw ore being regrinded after fragmentation accounts for 81.44%, the ore pulp that weight concentration is 38.79%; First in ore pulp, add inhibition zincblende and pyritous zinc sulfate solution and sodium sulfite aqueous solution, after fully stirring; In ore pulp, add respectively the amyl group sodium acrinol solution, 25 that galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral is combined to collecting more simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
Carried out the commerical test of 1 year 2000t/d by above-mentioned technological parameter, result shows to adopt above-mentioned technique and combined capturing and collecting agent administration condition can effectively carry the flotation recovery rate of high lead-antimony and associated silver, the plumbous antimony flow process of diffeential floatation of adopt one roughing, scan for three times, four times are selected, flotation of lead antimony mine tailing flotation zinc again.In the lead-antimony concentrate of obtaining in leaded 3.33%, antimony 1.05%, zinc 3.34%, sulphur 5.37%, silver-colored 163.45g/t, carbon content reach 1.52% ore pulp: lead adds antimony grade 59.09%, argentiferous 2257.16g/t, lead recovery 92.92%, antimony recovery 65.16%, silver raising recovery rate 88.31%.This embodiment is most preferred embodiment of the present invention.
Embodiment 3:
A kind of combined capturing and collecting agent, comprises amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 35:237:219.
When use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with to weight percent concentration and are 2.5% the aqueous solution, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add to respectively in ore pulp simultaneously.
The present invention is applied in a kind of method that adopts combined capturing and collecting agent raising antimony lead and associated silver flotation recovery rate, and the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous many metals of zinc antimony raw ore through broken, be ground to after mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate and the sodium sulfite that suppress zinc, sulfur mineral in ore pulp, after fully stirring; Add galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral are combined to the combined capturing and collecting agent of collecting, combination collecting obtains lead-antimony concentrate product.
Described fragmentation refers to the fine ore that plumbous many metals of zinc antimony crushing raw ore is less than to 12 millimeters to granularity; Described grinding refers to that adopting ore mill that granularity is less than to the fine ore of 12 millimeters is ground to after mineral disaggregation, forms the ore pulp that pH value is 7 ~ 7.5.
Zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; In combined capturing and collecting agent 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
The present invention is in the time of concrete application:
1, the former mineral material of the many metals of plumbous zinc antimony:
In the ore pulp forming: leaded 3.15%, antimony 0.94%, zinc 3.21%, sulphur 5.57%, silver-colored 144.17g/t, carbon content reach 1.61%; Pulp density 38.26%, a fineness-74 micron grade accounts for 81.73%; Plumbous antimony mainly exists with boulangerite and jamesonite form, and zinc is taking zincblende as main, and sulphur is taking pyrite and mispickel as main, and phosphorus content is higher, and fine particle stage material is than great.
2, floating agent and operating procedure:
Regime of agent:
By 1 ton of plumbous many metals of zinc antimony raw ore, in flotation: zinc sulfate consumption is 753g, sodium sulfite consumption is 165g, and amyl group sodium xanthate consumption is 35g, 25 #black powder consumption is 237g, and aerofloat 226 consumption is 219g.
When use, first medicament is mixed with to following weight percent concentration:
Zinc sulfate 5% aqueous solution
Sodium sulfite 5% aqueous solution
Amyl group sodium xanthate 2.5% aqueous solution
25 #black powder stoste is added
Aerofloat 226 2.5% aqueous solution;
Operating procedure:
Micron grade to fineness-74 of first plumbous many metals of zinc antimony raw ore being regrinded after fragmentation accounts for 810.73%, the ore pulp that weight concentration is 38.26%; First in ore pulp, add inhibition zincblende and pyritous zinc sulfate solution and sodium sulfite aqueous solution, after fully stirring; In ore pulp, add respectively the amyl group sodium acrinol solution, 25 that galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral is combined to collecting more simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
Carried out the commerical test of 1 year 2500t/d by above-mentioned technological parameter, result shows to adopt above-mentioned technique and combined capturing and collecting agent administration condition can effectively carry the flotation recovery rate of high lead-antimony and associated silver, the plumbous antimony flow process of diffeential floatation of adopt one roughing, scan for three times, four times are selected, flotation of lead antimony mine tailing flotation zinc again.In the lead-antimony concentrate of obtaining in leaded 3.15%, antimony 0.94%, zinc 3.21%, sulphur 5.57%, silver-colored 144.17g/t, carbon content reach 1.61% ore pulp: lead adds antimony grade 56.89%, argentiferous 2010.75g/t, lead recovery 94.44%, antimony recovery 65.78%, silver raising recovery rate 88.09%.
Embodiment 4:
A kind of combined capturing and collecting agent, comprises amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 20:200:150.
When use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with to weight percent concentration and are 5% the aqueous solution, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add to respectively in ore pulp simultaneously.
The present invention is applied in a kind of method that adopts combined capturing and collecting agent raising antimony lead and associated silver flotation recovery rate, and the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous many metals of zinc antimony raw ore through broken, be ground to after mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate and the sodium sulfite that suppress zinc, sulfur mineral in ore pulp, after fully stirring; Add galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral are combined to the combined capturing and collecting agent of collecting, combination collecting obtains lead-antimony concentrate product.
Described fragmentation refers to the fine ore that plumbous many metals of zinc antimony crushing raw ore is less than to 12 millimeters to granularity; Described grinding refers to that adopting ore mill that granularity is less than to the fine ore of 12 millimeters is ground to after mineral disaggregation, forms the ore pulp that pH value is 7 ~ 7.5.
Zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; In combined capturing and collecting agent 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
The present invention is in the time of concrete application:
1, the former mineral material of the many metals of plumbous zinc antimony:
In the ore pulp forming: leaded 3.15%, antimony 1.48%, zinc 3.75%, sulphur 5.73%, silver-colored 255.77g/t, carbon content reach 1.49%; Pulp density 39.54%, a fineness-74 micron grade accounts for 80.85%; Plumbous antimony mainly exists with boulangerite and jamesonite form, and zinc is taking zincblende as main, and sulphur is taking pyrite and mispickel as main, and phosphorus content is higher, and fine particle stage material is than great.
2, floating agent and operating procedure:
Regime of agent:
By 1 ton of plumbous many metals of zinc antimony raw ore, in flotation: zinc sulfate consumption is 400g, sodium sulfite consumption is 90g, and amyl group sodium xanthate consumption is 20g, 25 #black powder consumption is 200g, and aerofloat 226 consumption is 150g.
When use, first medicament is mixed with to following weight percent concentration:
Zinc sulfate 10% aqueous solution
Sodium sulfite 10% aqueous solution
Amyl group sodium xanthate 5% aqueous solution
25 #black powder stoste is added
Aerofloat 226 5% aqueous solution;
Operating procedure:
Micron grade to fineness-74 of first plumbous many metals of zinc antimony raw ore being regrinded after fragmentation accounts for 80.85%, the ore pulp that weight concentration is 39.54%; First in ore pulp, add inhibition zincblende and pyritous zinc sulfate solution and sodium sulfite aqueous solution, after fully stirring; In ore pulp, add respectively the amyl group sodium acrinol solution, 25 that galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral is combined to collecting more simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
Carried out the commerical test of 1 year 300t/d by above-mentioned technological parameter, result shows to adopt above-mentioned technique and combined capturing and collecting agent administration condition can effectively carry the flotation recovery rate of high lead-antimony and associated silver, the plumbous antimony flow process of diffeential floatation of adopt one roughing, scan for three times, four times are selected, flotation of lead antimony mine tailing flotation zinc again.In the lead-antimony concentrate of obtaining in leaded 3.15%, antimony 1.48%, zinc 3.75%, sulphur 5.73%, silver-colored 255.77g/t, carbon content reach 1.49% ore pulp: lead adds antimony grade 49.01%, argentiferous 3055.3g/t, lead recovery 78.15%, antimony recovery 64.44%, silver raising recovery rate 84.08%.
Embodiment 5:
A kind of combined capturing and collecting agent, comprises amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 21:250:190.
When use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with to weight percent concentration and are 2.5% the aqueous solution, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add to respectively in ore pulp simultaneously.
The present invention is applied in a kind of method that adopts combined capturing and collecting agent raising antimony lead and associated silver flotation recovery rate, and the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous many metals of zinc antimony raw ore through broken, be ground to after mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate and the sodium sulfite that suppress zinc, sulfur mineral in ore pulp, after fully stirring; Add galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral are combined to the combined capturing and collecting agent of collecting, combination collecting obtains lead-antimony concentrate product.
Described fragmentation refers to the fine ore that plumbous many metals of zinc antimony crushing raw ore is less than to 12 millimeters to granularity; Described grinding refers to that adopting ore mill that granularity is less than to the fine ore of 12 millimeters is ground to after mineral disaggregation, forms the ore pulp that pH value is 7 ~ 7.5.
Zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; In combined capturing and collecting agent 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
The present invention is in the time of concrete application:
1, the former mineral material of the many metals of plumbous zinc antimony:
In the ore pulp forming: leaded 3.15%, antimony 1.48%, zinc 3.75%, sulphur 5.73%, silver-colored 255.77g/t, carbon content reach 1.49%; Pulp density 39.54%, a fineness-74 micron grade accounts for 80.85%; Plumbous antimony mainly exists with boulangerite and jamesonite form, and zinc is taking zincblende as main, and sulphur is taking pyrite and mispickel as main, and phosphorus content is higher, and fine particle stage material is than great.
2, floating agent and operating procedure:
Regime of agent:
By 1 ton of plumbous many metals of zinc antimony raw ore, in flotation: zinc sulfate consumption is 700g, sodium sulfite consumption is 120g, and amyl group sodium xanthate consumption is 21g, 25 #black powder consumption is 250g, and aerofloat 226 consumption is 190g.
When use, first medicament is mixed with to following weight percent concentration:
Zinc sulfate 7% aqueous solution
Sodium sulfite 7% aqueous solution
Amyl group sodium xanthate 5% aqueous solution
25 #black powder stoste is added
Aerofloat 226 5% aqueous solution;
Operating procedure:
Micron grade to fineness-74 of first plumbous many metals of zinc antimony raw ore being regrinded after fragmentation accounts for 80.85%, the ore pulp that weight concentration is 39.54%; First in ore pulp, add inhibition zincblende and pyritous zinc sulfate solution and sodium sulfite aqueous solution, after fully stirring; In ore pulp, add respectively the amyl group sodium acrinol solution, 25 that galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral is combined to collecting more simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
Carried out the commerical test of 1 year 300t/d by above-mentioned technological parameter, result shows to adopt above-mentioned technique and combined capturing and collecting agent administration condition can effectively carry the flotation recovery rate of high lead-antimony and associated silver, the plumbous antimony flow process of diffeential floatation of adopt one roughing, scan for three times, four times are selected, flotation of lead antimony mine tailing flotation zinc again.In the lead-antimony concentrate of obtaining in leaded 3.15%, antimony 1.48%, zinc 3.75%, sulphur 5.73%, silver-colored 255.77g/t, carbon content reach 1.49% ore pulp: lead adds antimony grade 49.55%, argentiferous 3080.7g/t, lead recovery 78.66%, antimony recovery 65.09%, silver raising recovery rate 84.92%.
Embodiment 6:
A kind of combined capturing and collecting agent, comprises amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 50:350:300.
When use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with to weight percent concentration and are 1% the aqueous solution, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add to respectively in ore pulp simultaneously.
The present invention is applied in a kind of method that adopts combined capturing and collecting agent raising antimony lead and associated silver flotation recovery rate, and the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous many metals of zinc antimony raw ore through broken, be ground to after mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate and the sodium sulfite that suppress zinc, sulfur mineral in ore pulp, after fully stirring; Add galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral are combined to the combined capturing and collecting agent of collecting, combination collecting obtains lead-antimony concentrate product.
Described fragmentation refers to the fine ore that plumbous many metals of zinc antimony crushing raw ore is less than to 12 millimeters to granularity; Described grinding refers to that adopting ore mill that granularity is less than to the fine ore of 12 millimeters is ground to after mineral disaggregation, forms the ore pulp that pH value is 7 ~ 7.5.
Zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; In combined capturing and collecting agent 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
The present invention is in the time of concrete application:
1, the former mineral material of the many metals of plumbous zinc antimony:
In the ore pulp forming: leaded 3.33%, antimony 1.05%, zinc 3.34%, sulphur 5.37%, silver-colored 163.45g/t, carbon content reach 1.52%; Pulp density 38.79%, a fineness-74 micron grade accounts for 81.44%; Plumbous antimony mainly exists with boulangerite and jamesonite form, and zinc is taking zincblende as main, and sulphur is taking pyrite and mispickel as main, and phosphorus content is higher, and fine particle stage material is than great.
2, floating agent and operating procedure:
Regime of agent:
By 1 ton of plumbous many metals of zinc antimony raw ore, in flotation: zinc sulfate consumption is 1100g, sodium sulfite consumption is 180g, and amyl group sodium xanthate consumption is 50g, 25 #black powder consumption is 350g, and aerofloat 226 consumption is 300g.
When use, first medicament is mixed with to following weight percent concentration:
Zinc sulfate 5% aqueous solution
Sodium sulfite 5% aqueous solution
Amyl group sodium xanthate 1% aqueous solution
25 #black powder stoste is added
Aerofloat 226 1% aqueous solution;
Operating procedure:
Micron grade to fineness-74 of first plumbous many metals of zinc antimony raw ore being regrinded after fragmentation accounts for 81.44%, the ore pulp that weight concentration is 38.79%; First in ore pulp, add inhibition zincblende and pyritous zinc sulfate solution and sodium sulfite aqueous solution, after fully stirring; In ore pulp, add respectively the amyl group sodium acrinol solution, 25 that galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral is combined to collecting more simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
Carried out the commerical test of 1 year 2000t/d by above-mentioned technological parameter, result shows to adopt above-mentioned technique and combined capturing and collecting agent administration condition can effectively carry the flotation recovery rate of high lead-antimony and associated silver, the plumbous antimony flow process of diffeential floatation of adopt one roughing, scan for three times, four times are selected, flotation of lead antimony mine tailing flotation zinc again.In the lead-antimony concentrate of obtaining in leaded 3.33%, antimony 1.05%, zinc 3.34%, sulphur 5.37%, silver-colored 163.45g/t, carbon content reach 1.52% ore pulp: lead adds antimony grade 58.55%, argentiferous 2202.16g/t, lead recovery 91.77%, antimony recovery 64.56%, silver raising recovery rate 87.49%.

Claims (10)

1. a combined capturing and collecting agent, is characterized in that: comprise amyl group sodium xanthate, 25 #black powder and aerofloat 226; Described amyl group sodium xanthate, 25 #the part by weight of black powder and aerofloat 226 is: 2 ~ 5:20 ~ 35:15 ~ 30.
2. a kind of combined capturing and collecting agent according to claim 1, is characterized in that: when use, respectively amyl group sodium xanthate and aerofloat 226 are mixed with to weight percent concentration and are 1 ~ 5% the aqueous solution, and 25 #black powder is stoste; Amyl group sodium acrinol solution, 25 #black powder stoste and the aerofloat 226 aqueous solution are for add to respectively in ore pulp simultaneously.
3. a kind of method that adopts combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate according to claim 1, is characterized in that the method comprises the steps:
A, fragmentation, ore grinding:
By plumbous many metals of zinc antimony raw ore through broken, be ground to after mineral disaggregation, form ore pulp;
B, flotation:
First in ore pulp, add the zinc sulfate and the sodium sulfite that suppress zinc, sulfur mineral in ore pulp, after fully stirring; Add galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral are combined to the combined capturing and collecting agent of collecting, combination collecting obtains lead-antimony concentrate product.
4. a kind of method that adopts combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate according to claim 3, it is characterized in that: by 1 ton of plumbous many metals of zinc antimony raw ore, when flotation: zinc sulfate consumption is 400 ~ 1100g, sodium sulfite consumption is 90 ~ 180g, and combined capturing and collecting agent consumption is 370 ~ 700g.
5. a kind of method that adopts combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate according to claim 4, it is characterized in that: when use, respectively zinc sulfate and sodium sulfite are mixed with to weight percent concentration and are 5 ~ 10% the aqueous solution, respectively amyl group sodium xanthate and aerofloat 226 are mixed with again to weight percent concentration and are 1 ~ 5% the aqueous solution, and 25 #black powder is stoste; First in ore pulp, add the zinc sulfate solution and the sodium sulfite aqueous solution that suppress zinc, sulfur mineral, after fully stirring; In ore pulp, add respectively the amyl group sodium acrinol solution, 25 that galena, jamesonite, stibnite, silver-colored antimony tetrahedrite and associated silver mineral is combined to collecting more simultaneously #black powder stoste and the aerofloat 226 aqueous solution, combination collecting obtains lead-antimony concentrate product.
6. a kind of method that adopts combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate according to claim 3, is characterized in that: zinc sulfate and sodium sulfite are as the inhibitor of zinc, sulfur mineral; 25 #black powder and amyl group sodium xanthate are as the collecting agent of galena, jamesonite and stibnite, and aerofloat 226 is as the collecting agent of silver-colored antimony tetrahedrite and associated silver mineral.
7. a kind of method that adopts combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate according to claim 1, is characterized in that: amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 28:266:197.
8. a kind of method that adopts combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate according to claim 1, is characterized in that: amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 23:306:157.
9. a kind of method that adopts combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate according to claim 1, is characterized in that: amyl group sodium xanthate, 25 in described combined capturing and collecting agent #the part by weight of black powder and aerofloat 226 is: 35:237:219.
10. a kind of method that adopts combined capturing and collecting agent to improve antimony lead and associated silver flotation recovery rate according to claim 3, is characterized in that: described fragmentation refers to the fine ore that plumbous many metals of zinc antimony crushing raw ore is less than to 12 millimeters to granularity; Described grinding refers to that adopting ore mill that granularity is less than to the fine ore of 12 millimeters is ground to after mineral disaggregation, forms the ore pulp that pH value is 7 ~ 7.5.
CN201410121821.0A 2014-03-28 2014-03-28 Method for improving antimony, lead and associated silver flotation recovery rate by adopting combination collecting agent Active CN103831172B (en)