CN103506077A - 一种改性生物炭的制备方法 - Google Patents

一种改性生物炭的制备方法 Download PDF

Info

Publication number
CN103506077A
CN103506077A CN201310461243.0A CN201310461243A CN103506077A CN 103506077 A CN103506077 A CN 103506077A CN 201310461243 A CN201310461243 A CN 201310461243A CN 103506077 A CN103506077 A CN 103506077A
Authority
CN
China
Prior art keywords
charcoal
preparation
modification biological
biological charcoal
described step
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201310461243.0A
Other languages
English (en)
Inventor
江鸿
杨广西
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
University of Science and Technology of China USTC
Original Assignee
University of Science and Technology of China USTC
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by University of Science and Technology of China USTC filed Critical University of Science and Technology of China USTC
Priority to CN201310461243.0A priority Critical patent/CN103506077A/zh
Publication of CN103506077A publication Critical patent/CN103506077A/zh
Pending legal-status Critical Current

Abstract

一种改性生物炭的制备方法,其包括如下步骤:1)取适量生物炭,加入浓硫酸和浓硝酸的混合液,搅拌一段时间后进行过滤、水洗、烘干,得到硝化生物炭;2)向步骤1)中得到的硝化生物炭中加入水和还原剂,搅拌后进行升温回流处理,待反应物冷却后进行过滤、水洗、烘干,即获得改性生物炭。本发明的方法简易,易于工业化生产,制得的改性生物炭与现有生物炭或类生物炭吸附剂技术相比,对重金属的吸附性能大大提高,且具有相当的稳定性,吸附后解吸再生并可以重复使用。

Description

一种改性生物炭的制备方法
技术领域
本发明涉及生物炭吸附材料领域,特别涉及一种氨基修饰的改性生物炭的制备方法。
背景技术
我国每年有大量的诸如秸秆、稻壳之类的生物质遭到焚烧浪费,这不仅会给环境带来污染危害,还会造成生物能源的浪费和损失。近年来,随着热解技术逐步在我国推行,使得废弃生物质回收利用和能源再生得以实现。然而,在通过生物质热解技术获得可再生能源和化学品的同时,也产生了大批量的副产品--生物炭。如何充分而又合理地利用生物炭,如何使其变废为宝,这是需要人们亟待解决的问题,目前为止,生物炭被广泛应用在农业上,比如被用来土壤改良和土壤修复。此外,由于生物炭具有一定的分配作用和表面吸附作用,生物炭也逐渐被用作吸附剂,然而,生物炭本身表面吸附位点非常有限,所以其吸附性能和稳定性受到很大限制。因此,制备高吸附性能并且性质稳定的生物炭具有重要意义。
发明内容
有鉴于此,本发明的目在于提供一种吸附性能良好、稳定性高的氨基修饰改性生物炭的制备方法。
本发明提供的改性生物炭的制备方法,其包括如下步骤:
1)取适量生物炭,加入浓硫酸和浓硝酸的混合液,搅拌一段时间后进行过滤、水洗、烘干,得到硝化生物炭;
2)向步骤1)中得到的硝化生物炭中加入水和还原剂,搅拌后进行升温回流处理,待反应物冷却后进行过滤、水洗、烘干,即获得改性生物炭。
本发明方法所使用的生物炭采用本领域公知的方法制备,对其粒径没有特别要求,在具体实验操作中,可对生物炭进行筛分,选取40目~200目的生物炭进行实验。
在本发明方法的一个优选实施方案中,浓硫酸和浓硝酸的混合液起到对生物炭进行硝化的作用,其体积比优选为1:(1~5),生物炭的质量与浓硫酸和浓硝酸的混合液的体积的比优选为1:(10~50),其中生物炭的质量的单位为克,浓硫酸和浓硝酸的混合液的体积的单位为毫升。
在本发明方法的一个优选实施方案中,所述步骤1)中搅拌的时间为2h~6h,速率为200rpm~1000rpm。为了控制步骤1)中反应的温度,防止反应温度过高导致硝化效果不理想,所述步骤1)中搅拌还可在冰浴冷却的条件下进行。
在本发明的方法中,为了洗去硝化后生物炭中的有机杂质,步骤1)中的水洗后还可进行有机溶剂洗,其中有机溶剂可为异丙醇或乙醇等常见有机物。
在本发明方法的一个优选实施例中,所述步骤2)中的硝化生物炭和还原剂的质量比为1:(4~8)。
在本发明方法的一个优选实施例中,所述步骤2)中的还原剂选自连二亚硫酸钠、氯化亚锡或铁粉中的一种,其中连二亚硫酸钠因价格便宜为在工业中经常使用的还原剂,当还原剂为连二亚硫酸钠时,为了使用安全,步骤2)具体为:向步骤1)中得到的硝化生物炭中加入水、碱性溶液和连二亚硫酸钠,搅拌后加入酸并进行升温回流处理,待反应物冷却后进行过滤、水洗、烘干,即获得改性生物炭,碱性溶液优选自氨水或碳酸钠,酸优选自冰醋酸或盐酸。
在本发明方法的一个优选实施例中,所述步骤2)中搅拌的时间为5min~15min,速率为200rpm~1000rpm。
在本发明方法的一个优选实施例中,所述步骤2)中升温回流的温度为90℃~115℃,时间为4h~8h。在本发明中,“升温回流”是指对反应溶液进行加热,使溶剂变成蒸汽挥发后再冷凝流回反应溶液中。
在本发明的方法中,为了洗去硝化后生物炭中的有机杂质,步骤2)中的水洗后还可进行有机溶剂洗,其中有机溶剂可为异丙醇或乙醇等常见有机物。
本发明的方法的生物炭经硝化后得到硝化生物炭,再经还原得到改性特征炭,主要反应过程如下:R→R-NO2→R-NH2,其中R为生物炭。
本发明所制备的改性生物炭对于重金属废水处理有特别优良的效果,以金属铜离子为例,将改性生物炭投加到含铜溶液中,经传质作用,吸附很快达到平衡,铜离子被快速吸附去除,吸附后的改性生物炭可以通过酸液洗脱后回收再利用。
本发明的有益效果是:
(1)与现有生物炭或类生物炭吸附剂技术相比,本发明提供的改性生物炭对重金属的吸附性能大大提高;
(2)本发明提供的改性生物炭,是利用化学改性方法进行的改性,具有相当的稳定性,吸附后解吸再生并可以重复使用;
(3)本发明提供的制备方法简易,易于工业化生产。
附图说明
图1为S1与未改性生物炭的衰减全反射红外图,其中a为S1的衰减全反射红外图,b为未改性生物炭的衰减全反射红外图;
图2为S1与未改性生物炭的扫描电子显微镜照片,其中a为S1的扫描电子显微镜照片,b为未改性生物炭的扫描电子显微镜照片;
图3为S1与未改性生物炭对重金属铜离子的吸附动力学对比图;
图4为S1与未改性生物炭对重金属铜离子的截留保留能力对比图;
图5为S1受离子强度影响图;
图6为S2的等电点示意图。
具体实施方式
为使发明的上述目的、特征和优点能够更加明显易懂,下面对本发明的具体实施方式做详细的说明。
在下面的描述中阐述了很多具体细节以便于充分理解本发明,但是本发明还可以采用其他不同于在此描述的其它方式来实施,本领域技术人员可以在不违背本发明内涵的情况下做类似推广,因此本发明不受下面公开的具体实施例的限制。
本发明的实施例中所用的原料如下:
浓硫酸,分析纯,国药集团化学试剂有限公司
浓硝酸,分析纯,国药集团化学试剂有限公司
异丙醇,分析纯,国药集团化学试剂有限公司
氨水,质量分数26%,国药集团化学试剂有限公司
连二亚硫酸钠,化学纯,中国医药(集团)上海化学试剂公司
冰醋酸,分析纯,国药集团化学试剂有限公司
氢氧化钠,分析纯,国药集团化学试剂有限公司
本发明在实施例中采用常州普天仪器制造有限公司生产的JJ-1型精密增力电动搅拌器进行搅拌,采用合肥莎思腾博生化技术有限公司生产的iTC-10A型智能温度调节器进行升温回流实验,采用德国Bruker公司生产的VERTEX70FTIR光谱仪对生物炭的衰减全反射红外进行分析,采用美国FEI ElectronOptics公司生产的Sirion200扫描电镜对生物炭的形貌和尺寸进行检测,采用上海精密科学仪器有限公司生产的4530F型原子吸收分光光度计检测铜离子浓度,采用美国Micromeritics,Co.公司生产的ASAP2020M+C型的比表面分析仪检测生物炭的比表面积,采用德国Elementar vario公司生产的EL cube元素分析仪器检测生物炭的元素组成,采用瑞士Mettler-Toledo生产的DL50酸碱滴定仪检测生物炭的等电点。
实施例A1
a)将生物炭过60目筛后水洗、过滤、烘干;
b)取经a)步骤预处理过的生物炭3.0g,加入25mL浓硫酸和25mL浓硝酸的混合液,冰浴冷却下400rpm搅拌2h后过滤,滤饼水洗、异丙醇洗、烘干,得到硝化生物炭;
c)取硝化生物炭2.5g,加入25mL水、10mL氨水和14.0g连二亚硫酸钠,500rpm搅拌5min,然后加入60mL冰醋酸溶液,升温至100℃回流5h,冷却后过滤,滤饼水洗、异丙醇洗、烘干,即得到改性生物炭S1。
如图1所示,S1具有明显的氨基特征峰,及C-O官能团峰,未经改性生物炭不具备氨基、C-O官能团特征峰。
如图2所示,未改性生物炭表面具有明显的粗糙度和表面不规整性,而S1粗糙度和不规整性大大降低。
实施例A2
a)将生物炭过100目筛后水洗、过滤、烘干;
b)取经a)步骤预处理过的生物炭3.0g,加入15mL浓硫酸和30mL浓硝酸的混合液,冰浴冷却下500rpm搅拌4h后过滤,滤饼水洗、异丙醇洗、烘干,得到硝化生物炭;
c)取硝化生物炭2.5g,加入25mL水、10mL氨水和14.0g连二亚硫酸钠,700rpm搅拌5min,然后加入60mL冰醋酸溶液,升温至110℃回流8h,冷却后过滤,滤饼水洗、异丙醇洗、烘干,即得到改性生物炭S2。
如表1所示,S2和未改性生物炭的比表面积基本没有变化,且S2相对于未改性物炭富含大量的氮原子。
表1未改性生物炭和S2的BET检测和元素组成表
Figure BDA0000390819520000051
实施例B1
称取0.12g S1,加入40mL100ppm的铜溶液(含有0.01mol/L的NaNO3作为背景离子),用0.1mol/L硝酸调节pH至5,然后将样品放置在摇床中180转/分钟、30℃条件下震荡,每隔一定时间取样,过水系滤膜,然后测定滤液中铜浓度,对于未改性生物炭采取上述同样步骤以作为对比。
如图3所示,S1最大吸附容量是未改性生物炭的3倍,表明改性生物炭对重金属铜具有良好的吸附性能。
实施例B2
在两个相同的柱子中分别填充1.0g S1和未改性生物炭,在柱顶层加入少量石英砂,以防淋洗液将生物炭冲起,将25ppm的铜溶液从柱顶部加入,并用空气泵加压,保持铜溶液以2滴/秒的速度自柱底部流出,每间隔5mL收集流出液,将收集的流出液过水系滤膜,测定滤液中铜浓度,对于未改性生物炭采取上述同样步骤以作为对比。
如图4所示,S1对重金属铜溶液具有较好截留摄取能力。
实施例B3
称取三份0.12g S1,分别加入含有不同背景离子浓度的40mL100ppm的铜溶液(分别含有0.01mol/L、0.1mol/L和1mol/L的NaNO3作为背景离子),用0.1mol/L硝酸和0.1mol/L氢氧化钠调节溶液pH,然后将样品放置在摇床中180转/分钟、30℃条件下震荡,达到吸附平衡后取样,过水系滤膜,测定滤液中铜浓度。
如图5所示,S1吸附重金属过程中会受到背景离子强度的影响,而且离子强度越大,越不利于改性生物炭对重金属铜的去除,低的离子强度有利于重金属铜的去除。
实施例B4
称取16mg S2,加入40mL去离子水,用0.01mol/L的硝酸调节pH至2,然后将样品放置在酸碱滴定仪中,用0.01mol/L的NaOH进行滴定,记录溶液pH值的变化。
如图6所示,S2的等电点为3.9。
虽然本发明是结合以上实施例进行描述的,但本发明并不被限定于上述实施例,而只受所附权利要求的限定,本领域普通技术人员能够容易地对其进行修改和变化,但并不离开本发明的实质构思和范围。

Claims (10)

1.一种改性生物炭的制备方法,其特征在于,包括如下步骤:
1)取适量生物炭,加入浓硫酸和浓硝酸的混合液,搅拌一段时间后进行过滤、水洗、烘干,得到硝化生物炭;
2)向步骤1)中得到的硝化生物炭中加入水和还原剂,搅拌后进行升温回流处理,待反应物冷却后进行过滤、水洗、烘干,即获得改性生物炭。
2.根据权利要求1所述的改性生物炭的制备方法,其特征在于,所述步骤1)中的浓硫酸和浓硝酸的体积比为1:(1~5),生物炭的质量与浓硫酸和浓硝酸的混合液的体积的比为1:(10~50),其中生物炭的质量的单位为克,浓硫酸和浓硝酸的混合液的体积的单位为毫升。
3.根据权利要求1所述的改性生物炭的制备方法,其特征在于,所述步骤1)中搅拌的时间为2h~6h,速率为200rpm~1000rpm。
4.根据权利要求1所述的改性生物炭的制备方法,其特征在于,所述步骤1)中的搅拌在冰浴冷却的条件下进行。
5.根据权利要求1所述的改性生物炭的制备方法,其特征在于,所述步骤2)中的硝化生物炭和还原剂的质量比为1:(4~8)。
6.根据权利要求1所述的改性生物炭的制备方法,其特征在于,所述步骤2)中的还原剂选自连二亚硫酸钠、氯化亚锡或铁粉中的一种。
7.根据权利要求6所述的改性生物炭的制备方法,其特征在于,所述还原剂为连二亚硫酸钠时,步骤2)具体为:
向步骤1)中得到的硝化生物炭中加入水、碱性溶液和连二亚硫酸钠,搅拌后加入酸并进行升温回流处理,待反应物冷却后进行过滤、水洗、烘干,即获得改性生物炭。
8.根据权利要求7所述的改性生物炭的制备方法,其特征在于,所述步骤2)中的碱性溶液选自氨水或碳酸钠,酸选自冰醋酸或盐酸。
9.根据权利要求1所述的改性生物炭的制备方法,其特征在于,所述步骤2)中搅拌的时间为5min~15min,速率为200rpm~1000rpm。
10.根据权利要求1所述的改性生物炭的制备方法,其特征在于,所述步骤2)中升温回流的温度为90℃~115℃,时间为4h~8h。
CN201310461243.0A 2013-09-30 2013-09-30 一种改性生物炭的制备方法 Pending CN103506077A (zh)