CN103319130A - 一种建筑隔墙用轻质条板凹凸棒土粘结剂 - Google Patents
一种建筑隔墙用轻质条板凹凸棒土粘结剂 Download PDFInfo
- Publication number
- CN103319130A CN103319130A CN2013102120376A CN201310212037A CN103319130A CN 103319130 A CN103319130 A CN 103319130A CN 2013102120376 A CN2013102120376 A CN 2013102120376A CN 201310212037 A CN201310212037 A CN 201310212037A CN 103319130 A CN103319130 A CN 103319130A
- Authority
- CN
- China
- Prior art keywords
- parts
- attapulgite
- building partition
- binding agent
- partition wall
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
本发明公开了一种建筑隔墙用轻质条板凹凸棒土粘结剂,由以下重量份的原料组成:32.5快硬硫酸铝盐水泥120-150、纯丙乳液40-50、聚乙烯醇4-6、二甘醇3-4、羟乙基甲基纤维素2-3、石英砂100-150、植物纤维4-6、明矾石粉3-5、苯磺酰肼4-8、白云石粉5-10、凹凸棒土10-15、炉渣粉4-8、硼砂1-2、三乙醇胺5-8、3-氨丙基三甲氧基硅烷0.5-1。本发明建筑隔墙用轻质条板凹凸棒土粘结剂粘结力强,减少分层和剥落的机会,保障工程质量,避免长期使用后的空鼓、开裂等问题,从而提高耐久性。
Description
技术领域
本发明涉及一种建筑材料用粘结剂,具体涉及一种建筑隔墙用轻质条板凹凸棒土粘结剂。
背景技术
建筑隔墙用轻质条板是以普通硅酸盐水泥为胶凝材料,以陶粒、膨胀珍珠岩、工业灰渣等轻集料为主要原料,通过挤压成型而生产的多孔空心式条板。其施工安装时需要一定量的粘结剂固定。然而现有的粘结剂存在施工效率低、粘接性差、使用耐久性差以及安全性差等缺点,已经满足不了建筑隔墙用轻质条板的粘结要求。因此,急需研究开发一种全新高性能的建筑隔墙用轻质条板胶粘剂。
发明内容
本发明的目的在于针对现有技术的不足,提供一种粘结强度高、耐久性好、施工简单、安全无毒害的建筑隔墙用轻质条板凹凸棒土粘结剂。
本发明采用的技术方案如下:
一种建筑隔墙用轻质条板凹凸棒土粘结剂,由以下重量份的原料组成:
32.5快硬硫酸铝盐水泥 120-150
纯丙乳液 40-50
聚乙烯醇 4-6
二甘醇 3-4
羟乙基甲基纤维素 2-3
石英砂100-150
植物纤维 4-6
明矾石粉 3-5
苯磺酰肼 4-8
白云石粉 5-10
凹凸棒土 10-15
炉渣粉 4-8
硼砂1-2
三乙醇胺 5-8
3-氨丙基三甲氧基硅烷0.5-1。
优选地,一种建筑隔墙用轻质条板凹凸棒土粘结剂,由以下重量份的原料组成:
32.5快硬硫酸铝盐水泥 120
纯丙乳液 45
聚乙烯醇 5
二甘醇 3
羟乙基甲基纤维素 2
石英砂 140
植物纤维 5
明矾石粉 4
苯磺酰肼 6
白云石粉 8
凹凸棒土 10
炉渣粉 6
硼砂1.5
三乙醇胺 6
3-氨丙基三甲氧基硅烷0.8。
一种建筑隔墙用轻质条板凹凸棒土粘结剂的制备方法,包括以下步骤:
(1)将白云石粉和凹凸棒土混合均匀加入研磨机内,再加入硼砂、
三乙醇胺和3-氨丙基三甲氧基硅烷,2000-3000rpm高速研磨10-15分钟,取出烘干,粉碎研细,过50-100目筛,得白云石/凹凸棒土混合粉末,待用;
(2)将纯丙乳液加入到反应釜中,水浴加热至80-90℃,在搅拌下加入聚乙烯醇、二甘醇和羟乙基甲基纤维素,搅拌20-30分钟,再加入上述制得的白云石/凹凸棒土混合粉末继续搅拌10-15分钟,将乳液在250-280℃的热气流下进行喷雾干燥,得胶粉;
(3)将剩余原料与上述制得的胶粉干拌均匀,球磨1-2小时,过200-300目筛,装袋即可。
本发明的有益效果:
本发明建筑隔墙用轻质条板凹凸棒土粘结剂粘结力强,减少分层和剥落的机会,保障工程质量,避免长期使用后的空鼓、开裂等问题,从而提高耐久性;本发明胶粘剂预先干拌混合,质量稳定,使用时加入适量水的搅拌即可,施工简单方便;本发明有效利用炉渣粉等废料,无有毒有害添加物,完全符合环保要求,安全无污染。
具体实施方式
一种建筑隔墙用轻质条板凹凸棒土粘结剂,由以下重量份(千克)的原料组成:
32.5快硬硫酸铝盐水泥 120
纯丙乳液 45
聚乙烯醇 5
二甘醇 3
羟乙基甲基纤维素 2
石英砂 140
植物纤维 5
明矾石粉 4
苯磺酰肼 6
白云石粉 8
凹凸棒土 10
炉渣粉 6
硼砂1.5
三乙醇胺 6
3-氨丙基三甲氧基硅烷0.8。
一种建筑隔墙用轻质条板凹凸棒土粘结剂的制备方法,包括以下步骤:
(1)将白云石粉和凹凸棒土混合均匀加入研磨机内,再加入硼砂、
三乙醇胺和3-氨丙基三甲氧基硅烷,3000rpm高速研磨15分钟,取出烘干,粉碎研细,过80目筛,得白云石/凹凸棒土混合粉末,待用;
(2)将纯丙乳液加入到反应釜中,水浴加热至85℃,在搅拌下加入聚乙烯醇、二甘醇和羟乙基甲基纤维素,搅拌25分钟,再加入上述制得的白云石/凹凸棒土混合粉末继续搅拌15分钟,将乳液在260℃的热气流下进行喷雾干燥,得胶粉;
(3)将剩余原料与上述制得的胶粉干拌均匀,球磨1.5小时,过200目筛,装袋即可。
本发明粘结剂主要性能参数如下:
拉伸粘结强度(Mpa):1.1
浸水后的拉伸粘结强度(Mpa):0.9
热老化后的拉伸粘结强度(Mpa):0.8
冻融循环后的拉伸粘结强度(Mpa):0.6。
Claims (3)
1.一种建筑隔墙用轻质条板凹凸棒土粘结剂,其特征在于,由以下重量份的原料组成:
32.5快硬硫酸铝盐水泥 120-150
纯丙乳液 40-50
聚乙烯醇 4-6
二甘醇 3-4
羟乙基甲基纤维素 2-3
石英砂100-150
植物纤维 4-6
明矾石粉 3-5
苯磺酰肼 4-8
白云石粉 5-10
凹凸棒土 10-15
炉渣粉 4-8
硼砂1-2
三乙醇胺 5-8
3-氨丙基三甲氧基硅烷0.5-1。
2.根据权利要求1所述的一种建筑隔墙用轻质条板凹凸棒土粘结剂,其特征在于,由以下重量份的原料组成:
32.5快硬硫酸铝盐水泥 120
纯丙乳液 45
聚乙烯醇 5
二甘醇 3
羟乙基甲基纤维素 2
石英砂 140
植物纤维 5
明矾石粉 4
苯磺酰肼 6
白云石粉 8
凹凸棒土 10
炉渣粉 6
硼砂1.5
三乙醇胺 6
3-氨丙基三甲氧基硅烷0.8。
3.一种如权利要求1或2所述的建筑隔墙用轻质条板凹凸棒土粘结剂的制备方法,其特征在于包括以下步骤:
(1)将白云石粉和凹凸棒土混合均匀加入研磨机内,再加入硼砂、
三乙醇胺和3-氨丙基三甲氧基硅烷,2000-3000rpm高速研磨10-15分钟,取出烘干,粉碎研细,过50-100目筛,得白云石/凹凸棒土混合粉末,待用;
(2)将纯丙乳液加入到反应釜中,水浴加热至80-90℃,在搅拌下加入聚乙烯醇、二甘醇和羟乙基甲基纤维素,搅拌20-30分钟,再加入上述制得的白云石/凹凸棒土混合粉末继续搅拌10-15分钟,将乳液在250-280℃的热气流下进行喷雾干燥,得胶粉;
(3)将剩余原料与上述制得的胶粉干拌均匀,球磨1-2小时,过200-300目筛,装袋即可。