CN103184785A - 一种涂料施工工艺 - Google Patents

一种涂料施工工艺 Download PDF

Info

Publication number
CN103184785A
CN103184785A CN2011104428236A CN201110442823A CN103184785A CN 103184785 A CN103184785 A CN 103184785A CN 2011104428236 A CN2011104428236 A CN 2011104428236A CN 201110442823 A CN201110442823 A CN 201110442823A CN 103184785 A CN103184785 A CN 103184785A
Authority
CN
China
Prior art keywords
construction
paint
putty
coating
construction technology
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN2011104428236A
Other languages
English (en)
Other versions
CN103184785B (zh
Inventor
陈寿生
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Beijing Zhanchen Intelligent Property Management Co ltd
China Zhanchen New Materials Group Co.,Ltd.
Shanghai Zhanchen Paint Co ltd
Zhuhai Zhanchen New Material Co ltd
Original Assignee
Shanghai Fuchen Chemical Co Ltd
Beijing Zhanchen Chemical Co Ltd
Zhanchen Paint Group Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shanghai Fuchen Chemical Co Ltd, Beijing Zhanchen Chemical Co Ltd, Zhanchen Paint Group Co Ltd filed Critical Shanghai Fuchen Chemical Co Ltd
Priority to CN201110442823.6A priority Critical patent/CN103184785B/zh
Publication of CN103184785A publication Critical patent/CN103184785A/zh
Application granted granted Critical
Publication of CN103184785B publication Critical patent/CN103184785B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种涂料施工工艺,步骤主要包括:基面处理、腻子层施工、底漆层施工和面涂层施工,其特征在于,所述面漆层施工包括:使用2种以上不同颜色的涂料,间隔地平行平铺涂抹在墙面上,形成多个间隔的颜色带,再进行1次以上的刮批操作。本发明的施工工艺进行施工的墙面的面漆层能够达到非常特殊的艺术效果,特别是选用蓝色水性漆和白色水性漆进行施工时能够产生非常接近自然的“蓝天白云”的艺术效果;采用本发明的施工工艺施工的腻子层会达到非常好的平整度;本发明的施工工艺全部都优先采用水性漆,环保性好。

Description

一种涂料施工工艺
技术领域
本发明涉及涂料施工领域,特别涉及2种以上不同颜色涂料的施工工艺。
背景技术
近几年,随着建材市场的不断发展,人们对住宅楼、办公楼、商品楼等建筑物的装饰要求越来越高。
专利号为200510121176.3的专利公开了一种油漆涂装工艺,主要包括以下步骤:表面处理、上底色、中间效果处理及喷涂面漆。
传统涂料施工所采用的施工工艺都如上述专利公开的工艺一样,其技术效果为一道底漆加两道实色面漆的平面实色效果,颜色单一、形状单调,装饰效果差,不能满足日新月异的现代建筑物表面装饰的要求。
发明内容
本发明所要解决的技术问题就是克服现有技术的不足,提供一种能够产生良好的装饰效果的涂料施工工艺。
本发明解决其技术问题采用的技术方案是:
一种涂料施工工艺,步骤主要包括:基面处理、腻子层施工、底漆层施工和面涂层施工,所述面漆层施工包括:使用2种以上不同颜色的涂料,间隔地平行平铺涂抹在墙面上,形成多个间隔的颜色带,再进行1次以上的刮批操作。
优选的,所述的2种以上不同颜色的涂料都为水性涂料。
优选的,使用蓝色水性涂料和白色水性涂料这2种不同颜色的涂料,间隔地平行平铺涂抹在墙面上,形成多个蓝色和白色间隔的颜色带。
优选的,所述蓝色颜色带和白色颜色带的宽度比为1:2。
优选的,所述不同颜色带之间的距离为1-2mm。
优选的,所述的每次刮批操作之间对基面进行晾干操作,所述的晾干时间为5分钟。
优选的,进行2次刮批操作,第1次用不锈钢批刀进行刮批操作,第2次用软塑料批板进行刮批。
优选的,所述腻子层施工包括找平腻子找平、渗透粗腻子施工和修补细腻子施工。
与现有技术相比,本发明取得了以下的优越技术效果:采用本发明的施工工艺进行施工的墙面的面漆层能够达到非常特殊的艺术效果,特别是选用蓝色水性漆和白色水性漆进行施工时能够产生非常接近自然的“蓝天白云”的艺术效果;采用本发明的施工工艺施工的腻子层会达到非常好的平整度;本发明的施工工艺全部都优先采用水性漆,环保性好。
具体实施方式
本发明采用专用批刀对涂料进行批涂施工,在建筑物表面、混凝土、水泥砖石内、外墙及打过底的木材表面施工,步骤主要包括:基面处理、腻子层施工、底漆层施工和面涂层施工。
每一个施工步骤的具体内容如下:
1 基面处理:
    目的在于使得墙面平整,去除粘附物及浮尘。
1.1仔细检查墙面的平整度,将明显凹凸部位标出;
在实际实施过程中,本步骤使用2m长靠尺检查墙面平整度,采用彩色笔标出明显的凹凸部位;
1.2对有孔洞或明显的凹陷的部分用水泥砂浆进行修补;
1.3将明显的凸出部分和修补后的部位打磨至符合要求;
在实际实施过程中,采用砂轮机打磨打磨至≤2mm/2m;
1.4清除墙面粘附物及浮尘;
在实际实施过程中,用毛刷、铲刀及水等清除墙面粘附物及浮尘,也可以采用静电除尘。
2 腻子层施工:
    目的在于进一步提高墙面平整度,使其适合进行进一步的施工。在实际操作中,腻子层施工包括找平腻子找平、渗透粗腻子施工和修补细腻子施工:
2.1找平腻子找平:
2.1.1按照实际情况调配找平腻子;
在实际操作中,优先采用总督找平腻子VA6000和水10:1混合搅拌均匀,也可以采用其他找平腻子;
2.1.2满批找平腻子一道,干燥;
在实际操作中,找平腻子厚度在1mm左右,找平腻子的干燥操作采用晾干,晾干时间需要在12小时以上;
2.1.3再满批找平腻子一道,干燥;
在实际操作中,找平腻子厚度在1mm左右,找平腻子的干燥操作采用晾干,晾干时间需要在12小时以上。
2.2渗透粗腻子施工:
2.2.1按照实际情况调配渗透粗腻子;
实际操作中,优先采用总督双组份渗透粗腻子VA60001、固化剂VRH6001以及水按10:2:1的比例混合均匀,也可以采用其他单组份或双组份渗透粗腻子;
2.2.2满批渗透粗腻子;
2.2.3刮平,稍待干燥;
在实际操作中,稍待干燥操作采用晾干,晾干时间时间一般为3-4小时;
2.2.4砂磨,除去痕印;
2.2.5养护;
在实际操作中,为达到良好的施工效果,每次砂磨之后都进行养护,但也可以根据实际情况选择连续进行多次养护或跳过养护这个步骤;采用洒水养护,每次养护间隔时间为4小时,使得基面平整度≤1mm,表面无明显批刮印痕,无掉粉现象。;
再重复上述2.2.2至2.2.5步骤两次。
在实际操作中,第一次刮平采用刮尺由下至上刮平;第二刮平采用刮尺由左至右刮平;第三次刮平采用批刀收平;前两次砂磨采用使用40#砂纸或砂轮片打磨;第三次砂磨采用40#以上砂纸仔细砂磨,除去批刀印和接痕。
2.3修补细腻子施工:
2.3.1按照实际情况调配修补细腻子;
实际操作中,优先采用总督修补细腻子VR60002和水按10:1的比例搅拌均匀,还可以采用其他修补细腻子;
2.3.2满批修补细腻子一;
2.3.3刮平,稍待干燥;
实际操作中,采用批刀收平,稍待干燥操作采用晾干,晾干时间时间一般为3-4小时或干燥发白时即可;
2.3.4砂磨,除去痕印;
实际操作中,采用80#以上砂纸仔细砂磨;
2.3.5养护;
实际操作中,采用洒水养护,养护次数不少于4次,每次养护间隔4小时,使得平整度≤0.5mm,表面平滑,无任何批刮印痕;
2.3.6完全干燥;
实际操作中,干燥操作采用晾干,晾干时间48小时。
3底漆层施工:
3.1涂抹底漆;
实际操作中,采用滚筒滚涂,腻子层表面形成可见涂膜且无漏涂现象;底漆可以采用经典外墙全能抗碱白色底漆JWD9818或经典外墙水性白色封闭底漆VR28001,也可以采用其他水性或者油性的底漆;
3.2完全干燥;
实际操作中,干燥操作采用晾干,晾干时间12小时。
4面漆层施工:
4.1根据需要的分别调配2种以上不同颜色的涂料;
选用经典水性艺术白漆JWM5005作为第1种颜色的涂料;在经典水性艺术白漆JWM5005加入5%的水性蓝色色浆如科迪的6153-SA酞青兰或者CPS的BH2酞箐蓝充分搅拌均匀,调配成蓝色的水性艺术漆,作为第2种颜色的涂料。
在实际操作中,可以任意选择2种以上不同颜色的油性涂料和/或水性涂料;采用2种以上不同颜色的水性涂料会使得施工效果更好。
4.2将上述调配而成的2种以上不同颜色的涂料间隔地平行平铺涂抹在墙面上,形成多个间隔的颜色带,再进行1次以上的刮批操作;
将上述调配而成的蓝色水性艺术漆和在经典水性艺术白漆JWM5005间隔地平行平铺涂抹在墙面上,形成多个蓝色和白色间隔的颜色带,所述蓝色颜色带和白色颜色带的宽度比为1:2,相邻的颜色带之间的距离为1-2mm;用不锈钢批刀进行刮批操作,晾干时间5分钟后,再用软塑料批板进行刮批操作。
在实际操作中,根据实际情况和实际需要达到的艺术效果选择颜色带宽度比例和颜色带之间的距离,也可以根据实际情况选择别的刮批操作方式和/或别的刮批操作次数进行施工,多次刮批操作之间需要一定时间的干燥,根据刮批操作方式以及实际干燥程度来确定。
 
本施工工艺应在5℃以上,相对湿度小于85%的条件下施工;上述的干燥操作可以是晾干也可以是其他干燥方法,时间根据具体的干燥方法确定;还可以根据具体的情况和要求增加具有其他功能性或装饰性的中涂层或者罩面层。
与现有技术相比,本发明取得了以下的优越技术效果:采用本发明的施工工艺进行施工的墙面的面漆层能够达到非常特殊的艺术效果,特别是选用蓝色水性漆和白色水性漆进行施工时能够产生非常接近自然的“蓝天白云”的艺术效果;采用本发明的施工工艺施工的腻子层会达到非常好的平整度;本发明的施工工艺全部都优先采用水性漆,环保性好。 

Claims (8)

1.一种涂料施工工艺,步骤主要包括:基面处理、腻子层施工、底漆层施工和面涂层施工,其特征在于,所述面漆层施工包括:使用2种以上不同颜色的涂料,间隔地平行平铺涂抹在墙面上,形成多个间隔的颜色带,再进行1次以上的刮批操作。
2.根据权利要求1所述的施工工艺,其特征在于:所述的2种以上不同颜色的涂料都为水性涂料。
3.根据权利要求2所述的施工工艺,其特征在于:使用蓝色水性涂料和白色水性涂料这2种不同颜色的涂料,间隔地平行平铺涂抹在墙面上,形成多个蓝色和白色间隔的颜色带。
4.根据权利要求3所述的施工工艺,其特征在于:所述蓝色颜色带和白色颜色带的宽度比为1:2。
5.根据权利要求1至4任意一项所述的施工工艺,其特征在于:所述不同颜色带之间的距离为1-2mm。
6.根据权利要求1至4任意一项所述的施工工艺,其特征在于:所述的每次刮批操作之间对基面进行晾干操作,所述的晾干时间为5分钟。
7.根据权利要求6所述的施工工艺,其特征在于:进行2次刮批操作,第1次用不锈钢批刀进行刮批操作,第2次用软塑料批板进行刮批。
8.根据权利要求1所述的施工工艺,其特征在于:所述腻子层施工包括找平腻子找平、渗透粗腻子施工和修补细腻子施工。
CN201110442823.6A 2011-12-27 2011-12-27 一种涂料施工工艺 Active CN103184785B (zh)