A kind of production method of applying glue mica paper
Technical field
The present invention relates to a kind of mica paper production technology, particularly a kind of production method of applying glue mica paper.
Background technology
Mica is a kind of natural mineral matter, has excellent height insulation, withstands corona, acid and alkali-resistance, radiation-resistant effect.Mica generally in electrical industry, war products for making cable, giant mechanical and electrical equipment insulating materials, e.g., be pressed into the commutator mica sheet material of different-thickness, be processed into stamping parts using as the electric equipment such as generator, motor primary insulation parts.Mica capacitor has use in space flight, navigation, radar, and application category is extremely wide, is the indispensable high insulation in the world today, acid and alkali-resistance, heat-barrier material.
Research shows, mica is that a kind of natural mineral matter does not contain harmful material, but little by its scale radius-thickness ratio in machinery pulping process at mica, and fresh surface poor adhesive force, not easily passs through mica paper machine and directly become paper, becomes paper back pull poor, not easily rolling.
Summary of the invention
In order to overcome the defect of prior art, the invention provides a kind of production method of applying glue mica paper, it can improve adhesive force between scale, solves the defect of mica paper pulling force difference in process of production.
The technical solution used in the present invention is: a kind of production method of applying glue mica paper, its production stage is: first mica raw material is broken into mica magma through pulper, and mica magma is sent into stock tank of manufacturing paper with pulp, then by a certain amount of water of container splendid attire, be that the gelatine of 8 ° of E-12 ° of E is added to the water by viscosity, the gelatine quality added is the 15%-20% of quality, and heat with 70 DEG C of-90 DEG C of steams and make gelatine soluble in water, filter insoluble impurity through 90 order mesh screens and form gelatine solution, again by gelatine solution, defoamer add mica magma is housed manufacture paper with pulp in stock tank, and the amount of the gelatine solution added is 4 ‰-6 ‰ of mica magma gross mass in stock tank of manufacturing paper with pulp, the 0.005%-0.015% that the amount of defoamer is mica magma gross mass in stock tank of manufacturing paper with pulp, make mica magma and gelatine solution, defoamer mixes, manufacture paper with pulp shaping finally by mica paper machine, dry, qualified mica paper can be produced.
Being improved to further of such scheme, the total amount of described water is 34kg-36kg.
Being improved to further of such scheme, the model of described defoamer is JY-801.
Being improved to further of such scheme, described mica paper machine is 1092 cylinder mica paper machines.
Compared with prior art, the invention has the advantages that:
The present invention is by additional adhesive---and gelatine significantly can improve newborn lodicule surface adhesion force in mica paper production process, improve pulling force when mica paper is produced, to reduce disconnected paper when manufacturing paper with pulp, thus realize easily being wound into paper, improve paper machine speed, enhance productivity, effective reduction production cost, maintain again natural mica resistance to wear, high insulation, the advantage such as heat insulation, the mica paper produced is nontoxic, tasteless, cost performance is high, by being pressed into the commutator mica sheet material of different-thickness, be processed into stamping parts part, it is generator, the ideal basic material of the electric equipments such as motor.
Detailed description of the invention
Embodiment 1: first mica raw material is broken into mica magma through pulper, and mica magma is sent into stock tank of manufacturing paper with pulp, then by the water of container splendid attire 34kg, be that the gelatine of 8 ° of E is added to the water by viscosity, the gelatine quality added is 15% of quality, and heat with 70 DEG C of steams and make gelatine soluble in water, filter insoluble impurity through 90 order mesh screens and form gelatine solution, again by gelatine solution, defoamer (JY-801) add mica magma is housed manufacture paper with pulp in stock tank, and the amount of the gelatine solution added is 4 ‰ of mica magma gross mass in stock tank of manufacturing paper with pulp, the amount of defoamer is 0.005% of mica magma gross mass in stock tank of manufacturing paper with pulp, make mica magma and gelatine solution, defoamer mixes, manufacture paper with pulp shaping finally by mica paper machine, dry, namely qualified mica paper is produced.
Embodiment 2: first mica raw material is broken into mica magma through pulper, and mica magma is sent into stock tank of manufacturing paper with pulp, then by the water of container splendid attire 35kg, be that the gelatine of 10 ° of E is added to the water by viscosity, the gelatine quality added is 17.5% of quality, and heat with 80 DEG C of steams and make gelatine soluble in water, filter insoluble impurity through 90 order mesh screens and form gelatine solution, again by gelatine solution, defoamer add mica magma is housed manufacture paper with pulp in stock tank, and the amount of the gelatine solution added is 5 ‰ of mica magma gross mass in stock tank of manufacturing paper with pulp, the amount of defoamer is 0.01% of mica magma gross mass in stock tank of manufacturing paper with pulp, make mica magma and gelatine solution, defoamer mixes, manufacture paper with pulp shaping finally by mica paper machine, dry, namely qualified mica paper is produced.
Embodiment 3: first mica raw material is broken into mica magma through pulper, and mica magma is sent into stock tank of manufacturing paper with pulp, then by the water of container splendid attire 36kg, be that the gelatine of 12 ° of E is added to the water by viscosity, the gelatine quality added is 20% of quality, and heat with 90 DEG C of steams and make gelatine soluble in water, filter insoluble impurity through 90 order mesh screens and form gelatine solution, again by gelatine solution, defoamer (JY-801) add mica magma is housed manufacture paper with pulp in stock tank, and the amount of the gelatine solution added is 6 ‰ of mica magma gross mass in stock tank of manufacturing paper with pulp, the amount of defoamer is 0.015% of mica magma gross mass in stock tank of manufacturing paper with pulp, make mica magma and gelatine solution, defoamer mixes, manufacture paper with pulp shaping finally by 1092 cylinder mica paper machines on stock proportioner, dry, qualified mica paper can be produced.